CN105077806A - Decorating component for soft simulated bark and manufacturing method of decorating component - Google Patents

Decorating component for soft simulated bark and manufacturing method of decorating component Download PDF

Info

Publication number
CN105077806A
CN105077806A CN201410214869.6A CN201410214869A CN105077806A CN 105077806 A CN105077806 A CN 105077806A CN 201410214869 A CN201410214869 A CN 201410214869A CN 105077806 A CN105077806 A CN 105077806A
Authority
CN
China
Prior art keywords
mixture
silica gel
mesh
soft
weight
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201410214869.6A
Other languages
Chinese (zh)
Inventor
赵旋
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
SHENZHEN GREEN GRASS GARDENS LANDSCAPE CO Ltd
Original Assignee
SHENZHEN GREEN GRASS GARDENS LANDSCAPE CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by SHENZHEN GREEN GRASS GARDENS LANDSCAPE CO Ltd filed Critical SHENZHEN GREEN GRASS GARDENS LANDSCAPE CO Ltd
Priority to CN201410214869.6A priority Critical patent/CN105077806A/en
Publication of CN105077806A publication Critical patent/CN105077806A/en
Pending legal-status Critical Current

Abstract

The invention provides a decorating component for soft simulated bark. The decorating component is used for beautifying and bionic decorating of exposed portions of old trees, wall surfaces, column surfaces, water pipes, iron towers, handrails, simulated stumps, simulated wood, tree trunks, simulated trees and lampposts. The decorating component comprises at least one soft curing layer, each soft curing layer comprises silica gel, curing agent and meshed cloth, and each curing agent accounts for 1.5-3% of total weight of the corresponding silica gel. The invention further discloses a manufacturing method of the decorating component. The manufacturing method is easy in operation. The decorating component is high in simulation degree, plasticity, reducibility and weather resistance, long in service life and high in stability and wear resistance.

Description

A kind of decorative components of soft emulation bark and manufacture method thereof
Technical field
The present invention emulates bark and manufacture method thereof, particularly a kind of decorative components of soft emulation bark and manufacture method thereof.
Background technology
In natural landscape, primary trees are due to human factors such as natural cause and mismanagement such as thunder and lightning, insect pest, frosts, and vacancy, breakage appear in bark, and people need to utilize emulation bark to repair.
Lamp stand on communication base station, steel tower, highway, exposed in natural environment, people need to utilize emulation bark metallic iron tower, metal base station, metalized lamp rod are pretended and beautify.
In Landscape, have and many return ancient customs lattice bark roof, body of wall, railing, imitative wood, trunk, vacation tree, stub etc., due to true bark easily catch fire, insect pest, easily fungal infection, frangible, perishable, mouldability is poor, needs to utilize to emulate bark and decorate, replace.
Natural-bark easily catches fire, insect pest, easily fungal infection, frangible, perishable, mouldability is poor, and not easily peel off, can not be widely used in interior/exterior decoration and make scape, existing emulation bark is built with cement mostly, therefore it emulates bark fugitive color, easily comes off, fidelity is poor.
Summary of the invention
In order to solve above problem, the present invention proposes decorative components and the manufacture method thereof of the soft emulation bark that a kind of fidelity is high, weatherability is strong, anti-flammability is strong.
The technical program is achieved in that
The invention discloses a kind of decorative components of soft emulation bark, for the exposed portion of ancient tree, metope, cylinder, water pipe, steel tower, railing, imitative stub, imitative wood, trunk, artificial tree, lamp-stem beauty nature-imitation ornamental, comprise the soft cured layer of at least one deck, described soft cured layer comprises silica gel, curing agent, mesh class cloth, wherein, curing agent proportioning is 1.5% ~ 3% of silica gel gross weight.
In decorative components of the present invention, described soft cured layer also comprises silica, and the content (percentage by weight) of described silica is: 0.25% ~ 15% of described silica gel gross weight.
In decorative components of the present invention, soft cured layer also comprises look essence, and the content (percentage by weight) of described look essence is: 1% ~ 10% of described silica gel gross weight.
In decorative components of the present invention, described mesh dry goods, specifically comprises: mesh cloth, mesh chemical fabric, mesh cotton, mosquito netting, yarn cotton, Chopped Strand Mat.
The invention discloses a kind of method manufacturing above-mentioned decorative components, comprising:
S1. the die surface managed with artificial tree dermatoglyph is cleaned up, wiping is air-dry, then spray one deck oil-based release agent in mould texture face;
S2. the silica gel of liquid state is poured into container;
S3. be that 1.5% ~ 3% of silica gel gross weight joins in the container of silica gel by curing agent by proportioning, stir, obtain mixture;
S4. mixture is poured on equably mould texture aspect, with hairbrush, the mixture on die surface is fully brushed even in 1 ~ 20 minute, obtain the top layer of soft artificial tree skin decorating assembly; Wherein, mixture is poured on mould texture face and carries out according to 1.5 ~ 8.5KG/ square metre.
S5. in 1 ~ 60 minute at the non-grain layer upper berth mesh class cloth on the top layer of described soft artificial tree skin decorating assembly;
S6. on described mesh class cloth, go up mixture again, fully brushed even with hairbrush in 1 ~ 20 minute, make, in the mesh class cloth described in mixture immersion, fully to solidify to form an entirety with the non-grain layer on described soft artificial tree skin decorating assembly top layer; Wherein, mixture is poured on mould texture face and carries out according to 1.5 ~ 8.5KG/ square metre.
S7. in 15 ~ 240 minutes at normal temperatures, heat cure is shaping, the demoulding, obtains emulation bark.
In manufacture method of the present invention, also comprise step S22, add silica in described step S2 and S3, the content (percentage by weight) of described silica is: 0.25% ~ 15% of described silica gel gross weight.
In manufacture method of the present invention, in described step S2 and S3, also comprise step S23, add look essence, the content (percentage by weight) of described look essence is: 1% ~ 10% of described silica gel gross weight.
In manufacture method of the present invention, also comprise step S24, add silicone oil in described step S2 and S3, the content (percentage by weight) of described silicone oil is: 1% ~ 10% of described silica gel gross weight.
In manufacture method of the present invention, also comprise step S25, add fire retardant in described step S2 and S3, the content of described fire retardant accounts for mixture total weight amount percentage and is: 15% ~ 35%;
In manufacture method of the present invention, in described step S2 and S3, also comprise step S26, add stone flour class thing, the content of described stone flour class thing is the 1:0.5-1:2 of amount of the mixture; Affiliated stone flour mixture specifically comprises: stone flour, titanium dioxide, lithopone, forging white powder, the mixture of one or more do not come in powder, Malaysia powder.
In manufacture method of the present invention, after described step S7, also comprise step S8: the liniment adding 1 ~ 5% (percentage by weight) on the artificial tree dermatoglyph reason top layer of curing molding, carry out smearing art designing's process.
In manufacture method of the present invention, described liniment comprises: ink or R2000 solvent or oil modelled after an antique or their mixture.
In manufacture method of the present invention, described mesh dry goods, specifically comprises: mesh cloth, mesh chemical fabric, mesh cotton, mosquito netting, yarn cotton, Chopped Strand Mat.
Implement decorative components and the manufacture method thereof of a kind of soft emulation bark of the present invention, there is following useful technique effect:
Emulation bark of the present invention compensate for natural-bark easily infested, not easily peel off, the defect that interior/exterior decoration makes the uses such as scape can not be widely used in;
Improve emulation bark fugitive color that cement builds, easily come off, the defect of fidelity difference;
Emulation bark fidelity of the present invention is high, fugitive color, mouldable are strong by force, not for weatherability, and it is easy construction, cheap, fire-retardant energy is strong, can be widely used in ancient tree and repair, pretend and beautify steel tower, base station, lamp stand, finial, bag pillar, water pipe, lamp stand surface, wall body decoration etc.
Detailed description of the invention
Herein as there is no special declaration, be all weight percentage.
The invention discloses a kind of decorative components of soft emulation bark, for the exposed portion of ancient tree, metope, cylinder, water pipe, steel tower, railing, imitative stub, imitative wood, trunk, artificial tree, lamp-stem beauty nature-imitation ornamental, comprise the soft cured layer of at least one deck, soft cured layer comprises silica gel, curing agent, mesh class cloth, wherein, curing agent proportioning is 1.5% ~ 3% of silica gel gross weight.
Wherein, the water insoluble and any solvent of silica gel, nonpoisonous and tasteless, stable chemical nature, does not react with any material except highly basic, hydrofluoric acid, for doing the preferred of soft bark.
Curing agent, comprising: condensation polymer type two-component silicone rubber (RTV-2) crosslinking agent.
Mesh class cloth, comprising: mesh cloth, mesh chemical fabric, mesh cotton, mosquito netting, yarn cotton, Chopped Strand Mat etc., is convenient to decorative components and can forms block material shape.
Decorative components in the technical program can also comprise: silica, look essence.Their composition is:
The content (percentage by weight) of silica is: 0.25% ~ 15% of described silica gel gross weight.Adding silica is to prevent mixture from occurring deposited phenomenon.
The content (percentage by weight) of look essence is: 1% ~ 10% of described silica gel gross weight.
Look essence (premetallized dye is also transparency dye, is commonly called as look essence or toner, is a kind of dyestuff can using dissolution with solvents).
This decorative components can also add liniment, fire retardant, stone flour class thing, uv-resistant powder, antioxidant (264/1010/1076), UV resistant agent (UV-327, UV-329 etc.) or their mixture.
Wherein, the consumption of three kinds of compositions of uv-resistant powder, antioxidant (264/1010/1076), UV resistant agent (UV-327, UV-329 etc.) accounts for 0.2% ~ 0.5% of the total amount of decorative components.
Liniment comprises: (polymeric pigment of its Prof. Du Yucang, is invented the 1950's, is that pigment powder is in harmonious proportion acrylic based emulsion and makes for ink or R2000 solvent, acrylic paints.External pigment production producer has produced Propylene Series product, as sub-light acrylic paints, half sub-light acrylic paints and glossy acrylic paints and propylene semigloss oil, oil polish, plastotype ointment etc.) and oil modelled after an antique or their mixture.
Stone flour class thing, specifically comprises: stone flour, titanium dioxide, lithopone, forging white powder, the mixture of one or more do not come in powder, Malaysia powder, and adding stone flour class thing is to prevent mixture excessively rare.
Further, fire retardant comprises: MCA or TCEP.The content (percentage by weight) of described fire retardant can be: in the silica gel of 75-85 kilogram and the mixture of silicone oil, add the fire retardant of 35-15 kilogram.Or in the silica gel of 75-85 kilogram, add the fire retardant of 35-15 kilogram.Or in the silica gel of 75-85 kilogram, silica mixture, add the fire retardant of 35-15 kilogram.Or in the silica gel of 75-85 kilogram, silica, silicon oil mixture, add the fire retardant of 35-15 kilogram.Or in the silica gel of 75-85 kilogram, silica, silicone oil, stone flour mixture, add the fire retardant of 35-15 kilogram.Or in the silica gel of 75-85 kilogram, silica, silicone oil, stone flour, look essence mixture, add the fire retardant of 35-15 kilogram.
Embodiment one,
S1. the die surface with simulant grain is cleaned up, wiping is air-dry, then spray one deck oil-based release agent in mould texture face;
S2. getting weight is that the silica gel of the liquid state of 50Kg is poured in container;
S3. the curing agent of 0.75KG is joined in the container of silica gel, stir, obtain mixture;
S4. mixture is poured on equably mould texture face, with hairbrush, the mixture on die surface is fully brushed even in 3 minutes, obtain the top layer of soft artificial tree skin decorating assembly; Wherein, mixture is poured on mould texture face and carries out according to 1.5KG/ square metre.
S5. in 8 minutes at the non-grain layer upper berth glass-fiber-fabric on the top layer of described soft artificial tree skin decorating assembly;
S6. on described glass-fiber-fabric, go up mixture again, fully brushed even with hairbrush in 3 minutes, make fully to solidify to form an entirety with the non-grain layer on described soft artificial tree skin decorating assembly top layer in the glass-fiber-fabric described in mixture immersion; Wherein, mixture is poured on mould texture face and carries out according to 1.5KG/ square metre.
S7. in 30 minutes at normal temperatures, heat cure is shaping, the demoulding, obtains emulation bark.
Embodiment two,
S1. the die surface with simulant grain is cleaned up, wiping is air-dry, then spray one deck oil-based release agent in mould texture face;
S2. getting weight is that the silica gel of the liquid state of 100Kg imports in container;
S21. being added by the silica of 1Kg has in the container of silica gel, stirs, obtains the first mixture;
S3. in the first mixture, add the curing agent of 1.7Kg, stir, obtain the second mixture;
S4. the second mixture is poured on mould texture face equably, with hairbrush, the second mixture on die surface is fully brushed even in 5 minutes, obtain the top layer of soft artificial tree skin decorating assembly; Wherein, the second mixture is poured on mould texture face and carries out according to 4.5KG/ square metre.
S5. in 10 minutes at the non-grain layer upper berth Chopped Strand Mat on the top layer of described soft artificial tree skin decorating assembly;
S6. on Chopped Strand Mat, go up the second mixture again, fully brushed even with hairbrush in 6 minutes, the second mixture is immersed in Chopped Strand Mat and fully solidify to form an entirety with the non-grain layer on described soft artificial tree skin decorating assembly top layer; Wherein, the second mixture is poured on mould texture face and carries out according to 4.5KG/ square metre.
S7. in 60 minutes at normal temperatures, heat cure is shaping, the demoulding, obtains emulation bark.
Embodiment three,
S1. the die surface with simulant grain is cleaned up, wiping is air-dry, then spray one deck oil-based release agent in mould texture face;
S2. getting weight is that the silica gel of the liquid state of 150Kg is put in container;
S21. the silica of 5Kg is joined in the container of silica gel, stir, obtain the first mixture;
S22. the look essence of 2Kg is joined the first mixture, stir, obtain the second mixture;
S3. in the second mixture, add the curing agent of 2.5Kg, stir, obtain the 3rd mixture;
S4. the 3rd mixture is poured on mould texture face equably, with hairbrush, the 3rd mixture on die surface is fully brushed even in 20 minutes, obtain the top layer of soft artificial tree skin decorating assembly; Wherein, the 3rd mixture is poured on mould texture face and carries out according to 5KG/ square metre.
S5. in 20 minutes at the non-grain layer upper berth mesh cotton on the top layer of described soft artificial tree skin decorating assembly;
S6. on described mesh cotton, go up the 3rd mixture again, fully brushed even with hairbrush in 16 minutes, make fully to solidify to form an entirety with the non-grain layer on described soft artificial tree skin decorating assembly top layer in the mesh cotton described in the 3rd mixture immersion; Wherein, the 3rd mixture is poured on mould texture face and carries out according to 5KG/ square metre.
S7. in 120 minutes at normal temperatures, heat cure is shaping, the demoulding, obtains emulation bark.
Embodiment four,
S1. the die surface with simulant grain is cleaned up, wiping is air-dry, then spray one deck oil-based release agent in mould texture face;
S2. getting weight is that container poured into by the silica gel of the liquid state of 250Kg;
S21. the silica of 25Kg is joined in the container of silica gel, stir, obtain the first mixture;
S22. the look essence of 20Kg is joined the first mixture, stir, obtain the second mixture;
S3. in the second mixture, add the curing agent of 5.25Kg, stir, obtain the 3rd mixture;
S4. the 3rd mixture is poured on mould texture face equably, with hairbrush, the 3rd mixture on die surface is fully brushed even in 20 minutes, obtain the top layer of soft artificial tree skin decorating assembly; Wherein, the 3rd mixture is poured on mould texture face and carries out according to 7KG/ square metre.
S5. in 45 minutes at the non-grain layer upper berth mesh chemical fabric on the top layer of described soft artificial tree skin decorating assembly;
S6. go up the 3rd mixture again at mesh chemical fabric, fully brushed even with hairbrush in 15 minutes, make the non-grain layer that the 3rd mixture immerses mesh chemical fabric and described soft artificial tree skin decorating assembly top layer fully solidify to form an entirety; Wherein, the 3rd mixture is poured on mould texture face and carries out according to 8KG/ square metre.
S7. in 180 minutes at normal temperatures, heat cure is shaping, the demoulding, obtains emulation bark.
Embodiment five,
S1. the die surface with simulant grain is cleaned up, wiping is air-dry, then spray one deck oil-based release agent in mould texture face;
S2. getting weight is that container poured into by the silica gel of the liquid state of 200Kg;
S21. the silica of 12Kg is joined in the container of silica gel, stir, obtain the first mixture;
S22. the look essence of 13Kg is joined the first mixture, stir, obtain the second mixture;
S23. in the second mixture, add the silicone oil of 3Kg, stir, obtain the 3rd mixture;
S3. in the 3rd mixture, add the curing agent of 5.0Kg, stir, obtain 4 mixture;
S4. 4 mixture is poured on mould texture face equably, with hairbrush, the 4 mixture on die surface is fully brushed even in 20 minutes, obtain the top layer of soft artificial tree skin decorating assembly; Wherein, 4 mixture is poured on mould texture face and carries out according to 7KG/ square metre.
S5. in 45 minutes at the non-grain layer upper berth mesh chemical fabric on the top layer of described soft artificial tree skin decorating assembly;
S6. go up 4 mixture again at mesh chemical fabric, fully brushed even with hairbrush in 20 minutes, make the non-grain layer that 4 mixture immerses mesh chemical fabric and described soft artificial tree skin decorating assembly top layer fully solidify to form an entirety; Wherein, 4 mixture is poured on mould texture face and carries out according to 8.5KG/ square metre.
S7. in 200 minutes at normal temperatures, heat cure is shaping, the demoulding, obtains emulation bark.
Embodiment six,
S1. the die surface with simulant grain is cleaned up, wiping is air-dry, then spray one deck oil-based release agent in mould texture face;
S2. getting weight is that container poured into by the silica gel of the liquid state of 500Kg;
S21. the silica of 75Kg is joined in the container of silica gel, stir, obtain the first mixture;
S22. the look essence of 50Kg is joined the first mixture, stir, obtain the second mixture;
S23. in the second mixture, add the silicone oil of 50Kg, stir, obtain the 3rd mixture;
S24. in the 3rd mixture, add the fire retardant of 125Kg, stir, obtain 4 mixture;
S3. the curing agent of 15Kg is joined in 4 mixture, stir, obtain the 5th mixture;
S4. the 5th mixture is poured on mould texture face equably, with hairbrush, the 5th mixture on die surface is fully brushed even in 20 minutes, obtain the top layer of soft artificial tree skin decorating assembly; Wherein, the 5th mixture is poured on mould texture face and carries out according to 7KG/ square metre.
S5. in 50 minutes at the non-grain layer upper berth mesh chemical fabric on the top layer of described soft artificial tree skin decorating assembly;
S6. go up the 5th mixture again at mesh chemical fabric, fully brushed even with hairbrush in 19 minutes, make the non-grain layer that the 5th mixture immerses mesh chemical fabric and described soft artificial tree skin decorating assembly top layer fully solidify to form an entirety; Wherein, the 5th mixture is poured on mould texture face and carries out according to 8.5KG/ square metre.
S7. in 230 minutes at normal temperatures, heat cure is shaping, the demoulding, obtains emulation bark.
With the ink of 6Kg on the surface of the emulation bark perithelium layer S8. obtained after demoulding, smear art designing's process uniformly.
Stone flour class thing, uv-resistant powder, antioxidant (264/1010/1076), UV resistant agent (UV-327, UV-329 etc.) or their mixture can also be added in the manufacture method of this decorative components.
Wherein, the consumption of three kinds of compositions of uv-resistant powder, antioxidant (264/1010/1076), UV resistant agent (UV-327, UV-329 etc.) accounts for the 0.2%-0.5% of the total amount of decorative components.
Stone flour class thing, specifically comprises: stone flour, titanium dioxide, lithopone, forging white powder, the mixture of one or more do not come in powder, Malaysia powder.
Liniment comprises: (polymeric pigment of its Prof. Du Yucang, is invented the 1950's, is that pigment powder is in harmonious proportion acrylic based emulsion and makes for ink or R2000 solvent, acrylic paints.External pigment production producer has produced Propylene Series product, as sub-light acrylic paints, half sub-light acrylic paints and glossy acrylic paints and propylene semigloss oil, oil polish, plastotype ointment etc.) and oil modelled after an antique or their mixture.
Embodiment seven,
S1. the die surface with simulant grain is cleaned up, wiping is air-dry, then spray one deck oil-based release agent in mould texture face;
S2. getting weight is that container poured into by the silica gel of the liquid state of 600Kg;
S21. the silica of 1.5Kg is joined in the container of silica gel, stir, obtain the first mixture;
S22. the look essence of 6Kg is joined the first mixture, stir, obtain the second mixture;
S23. in the second mixture, add the silicone oil of 6Kg, stir, obtain the 3rd mixture;
S24. in the 3rd mixture, add the fire retardant of 90Kg, stir, obtain 4 mixture;
S25. the stone flour of 360Kg is joined in 4 mixture, stir, obtain the 5th mixture;
S3. the curing agent of 9Kg is joined in the 5th mixture, stir, obtain the 6th mixture;
S4. the 6th mixture is poured on mould texture face equably, with hairbrush, the 6th mixture on die surface is fully brushed even in 5 minutes, obtain the top layer of soft artificial tree skin decorating assembly; Wherein, the 6th mixture is poured on mould texture face and carries out according to 1.8KG/ square metre.
S5. in 10 minutes at the non-grain layer upper berth mesh chemical fabric on the top layer of described soft artificial tree skin decorating assembly;
S6. go up the 6th mixture again at mesh chemical fabric, fully brushed even with hairbrush in 6 minutes, make the non-grain layer that the 6th mixture immerses mesh chemical fabric and described soft artificial tree skin decorating assembly top layer fully solidify to form an entirety; Wherein, the 6th mixture is poured on mould texture face and carries out according to 2.0KG/ square metre.
S7. in 30 minutes at normal temperatures, heat cure is shaping, the demoulding, obtains emulation bark.
With the ink of 6.5Kg on the surface of the emulation bark perithelium layer S8. obtained after demoulding, smear art designing's process uniformly.
Embodiment eight,
S1. the die surface with simulant grain is cleaned up, wiping is air-dry, then spray one deck oil-based release agent in mould texture face;
S2. getting weight is that container poured into by the silica gel of the liquid state of 800Kg;
S21. the silica of 64Kg is joined in the container of silica gel, stir, obtain the first mixture;
S22. the look essence of 40Kg is joined the first mixture, stir, obtain the second mixture;
S23. in the second mixture, add the silicone oil of 40Kg, stir, obtain the 3rd mixture;
S24. in the 3rd mixture, add the fire retardant of 160Kg, stir, obtain 4 mixture;
S25. the titanium dioxide of 1000Kg is joined in 4 mixture, stir, obtain the 5th mixture;
S3. the curing agent of 16Kg is joined in the 5th mixture, stir, obtain the 6th mixture;
S4. the 6th mixture is poured on mould texture face equably, with hairbrush, the 6th mixture on die surface is fully brushed even in 12 minutes, obtain the top layer of soft artificial tree skin decorating assembly; Wherein, the 6th mixture is poured on mould texture face and carries out according to 4.5KG/ square metre.
S5. in 40 minutes at the non-grain layer upper berth mesh chemical fabric on the top layer of described soft artificial tree skin decorating assembly;
S6. go up the 6th mixture again at mesh chemical fabric, fully brushed even with hairbrush in 15 minutes, make the non-grain layer that the 6th mixture immerses mesh chemical fabric and described soft artificial tree skin decorating assembly top layer fully solidify to form an entirety; Wherein, the 6th mixture is poured on mould texture face and carries out according to 4.0KG/ square metre.
S7. in 200 minutes at normal temperatures, heat cure is shaping, the demoulding, obtains emulation bark.
With the ink of 20Kg on the surface of the emulation bark perithelium layer S8. obtained after demoulding, smear art designing's process uniformly.
Embodiment nine,
S1. the die surface with simulant grain is cleaned up, wiping is air-dry, then spray one deck oil-based release agent in mould texture face;
S2. getting weight is that container poured into by the silica gel of the liquid state of 1000Kg;
S21. the silica of 150Kg is joined in the container of silica gel, stir, obtain the first mixture;
S22. the look essence of 100Kg is joined the first mixture, stir, obtain the second mixture;
S23. in the second mixture, add the silicone oil of 100Kg, stir, obtain the 3rd mixture;
S24. in the 3rd mixture, add the fire retardant of 350Kg, stir, obtain 4 mixture;
S25. the Malaysia powder of 4000Kg is joined in 4 mixture, stir, obtain the 5th mixture;
S3. the curing agent of 30Kg is joined in the 5th mixture, stir, obtain the 6th mixture;
S4. the 6th mixture is poured on mould texture face equably, with hairbrush, the 6th mixture on die surface is fully brushed even in 18 minutes, obtain the top layer of soft artificial tree skin decorating assembly; Wherein, the 6th mixture is poured on mould texture face and carries out according to 8.1KG/ square metre.
S5. in 57 minutes at the non-grain layer upper berth mesh chemical fabric on the top layer of described soft artificial tree skin decorating assembly;
S6. go up the 6th mixture again at mesh chemical fabric, fully brushed even with hairbrush in 20 minutes, make the non-grain layer that the 6th mixture immerses mesh chemical fabric and described soft artificial tree skin decorating assembly top layer fully solidify to form an entirety; Wherein, the 6th mixture is poured on mould texture face and carries out according to 8.0KG/ square metre.
S7. in 235 minutes at normal temperatures, heat cure is shaping, the demoulding, obtains emulation bark.
With the ink of 50Kg on the surface of the emulation bark perithelium layer S8. obtained after demoulding, smear art designing's process uniformly.

Claims (13)

1. the decorative components of a soft emulation bark, for the exposed portion of ancient tree, metope, cylinder, water pipe, steel tower, railing, imitative stub, imitative wood, trunk, artificial tree, lamp-stem beauty nature-imitation ornamental, it is characterized in that, comprise the soft cured layer of at least one deck, described soft cured layer comprises silica gel, curing agent, mesh class cloth, wherein, curing agent proportioning is 1.5% ~ 3% of silica gel gross weight.
2. decorative components according to claim 1, is characterized in that, described soft cured layer also comprises silica, and the content (percentage by weight) of described silica is: 0.25% ~ 15% of described silica gel gross weight.
3. decorative components according to claim 1, is characterized in that, soft cured layer also comprises look essence, and the content (percentage by weight) of described look essence is: 1% ~ 10% of described silica gel gross weight.
4. decorative components according to claim 1, is characterized in that, described mesh dry goods, specifically comprises: mesh cloth, mesh chemical fabric, mesh cotton, mosquito netting, yarn cotton, Chopped Strand Mat.
5. a method for the decorative components described in manufacturing claims 1, is characterized in that, comprising:
S1. the die surface managed with artificial tree dermatoglyph is cleaned up, wiping is air-dry, then spray one deck oil-based release agent in mould texture face;
S2. the silica gel of liquid state is poured into container;
S3. be that 1.5% ~ 3% of silica gel gross weight joins in the container of silica gel by curing agent by proportioning, stir, obtain mixture;
S4. mixture is poured on equably mould texture aspect, with hairbrush, the mixture on die surface is fully brushed even in 1 ~ 20 minute, obtain the top layer of soft artificial tree skin decorating assembly; Wherein, mixture is poured on mould texture face and carries out according to 1.5 ~ 8.5KG/ square metre.
S5. in 1 ~ 60 minute at the non-grain layer upper berth mesh class cloth on the top layer of described soft artificial tree skin decorating assembly;
S6. on described mesh class cloth, go up mixture again, fully brushed even with hairbrush in 1 ~ 20 minute, make, in the mesh class cloth described in mixture immersion, fully to solidify to form an entirety with the non-grain layer on described soft artificial tree skin decorating assembly top layer; Wherein, mixture is poured on mould texture face and carries out according to 1.5 ~ 8.5KG/ square metre.
S7. in 15 ~ 240 minutes at normal temperatures, heat cure is shaping, the demoulding, obtains emulation bark.
6. manufacture method according to claim 5, it is characterized in that, in described step S2 and S3, also comprise step S22, add silica, the content (percentage by weight) of described silica is: 0.25% ~ 15% of described silica gel gross weight.
7. the manufacture method according to any one of claim 5 or 6, it is characterized in that, in described step S2 and S3, also comprise step S23, add look essence, the content (percentage by weight) of described look essence is: 1% ~ 10% of described silica gel gross weight.
8. manufacture method according to claim 7, is characterized in that, also comprises step S24, add silicone oil in described step S2 and S3, and the content (percentage by weight) of described silicone oil is: 1% ~ 10% of described silica gel gross weight.
9. manufacture method according to claim 8, is characterized in that, also comprises step S25, add fire retardant in described step S2 and S3, and the content of described fire retardant accounts for mixture total weight amount percentage and is: 15% ~ 35%.
10. manufacture method according to claim 9, it is characterized in that, also step S26 is comprised in described step S2 and S3, add 1:0.5 ~ 1:2 that stone flour class thing is the gross weight of mixture after adding fire retardant, described stone flour class thing comprises: stone flour, titanium dioxide, lithopone, forging white powder, the mixture of one or more do not come in powder, Malaysia powder.
11. manufacture methods according to claim 10, it is characterized in that, after described step S7, also comprise step S8: the liniment adding 1 ~ 5% (percentage by weight) on the artificial tree dermatoglyph reason top layer of curing molding, carry out smearing art designing's process.
12. manufacture methods according to claim 11, is characterized in that, described liniment comprises: ink or R2000 solvent or oil modelled after an antique or their mixture.
13. manufacture methods according to claim 5, is characterized in that, described mesh dry goods, specifically comprises: mesh cloth, mesh chemical fabric, mesh cotton, mosquito netting, yarn cotton, Chopped Strand Mat.
CN201410214869.6A 2014-05-21 2014-05-21 Decorating component for soft simulated bark and manufacturing method of decorating component Pending CN105077806A (en)