CN104924396A - Thorn softening method - Google Patents

Thorn softening method Download PDF

Info

Publication number
CN104924396A
CN104924396A CN201510285556.4A CN201510285556A CN104924396A CN 104924396 A CN104924396 A CN 104924396A CN 201510285556 A CN201510285556 A CN 201510285556A CN 104924396 A CN104924396 A CN 104924396A
Authority
CN
China
Prior art keywords
parts
twigs
chaste tree
treatment fluid
water
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201510285556.4A
Other languages
Chinese (zh)
Inventor
李明
李东猛
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
FUNAN COUNTY MENGFA ARTS & CRAFTS Co Ltd
Original Assignee
FUNAN COUNTY MENGFA ARTS & CRAFTS Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by FUNAN COUNTY MENGFA ARTS & CRAFTS Co Ltd filed Critical FUNAN COUNTY MENGFA ARTS & CRAFTS Co Ltd
Priority to CN201510285556.4A priority Critical patent/CN104924396A/en
Publication of CN104924396A publication Critical patent/CN104924396A/en
Pending legal-status Critical Current

Abstract

The invention relates to a thorn softening method. The method comprises the following steps: (1) conditioning fluid A is prepared; (2) thorns are dipped for 18 h at a temperature of 42 DEG C by using the conditioning fluid, and are fished out for weaving; and (3) conditioning fluid B is used for conditioning; 68 parts of water and 4 parts of polyethylene glycol are stirred at a temperature of 42-45 DEG C for fully dissolving; then, the woven thorn products are dipped therein for 2 h; and then, 4.6 parts of sodium bicarbonate and 2.4 parts of sodium salicylate are added for dissolving, are continuously dipped for 3 h, are fished out, and are cleaned by clear water. The thorn softening method, provided by the invention, is simple; and the thorns can be softened before being woven, so that the weaving difficulty is reduced, and the cracking or the rupture of the thorns is prevented in the weaving process.

Description

A kind of twigs of the chaste tree softening method
Technical field
The invention belongs to treating of wood field, be specifically related to a kind of twigs of the chaste tree softening method.
Background technology
The twigs of the chaste tree, be a kind of important wicker plaiting article raw material, the twigs of the chaste tree are more tough and tensile, carry out sofening treatment be then difficult to weave if do not added, not only easily cause the twigs of the chaste tree to ftracture even to fracture, cause the outward appearance of goods unsightly, and cause the firmness of twigs of the chaste tree goods and corrosion resistance to reduce, existing also have use softening method before braiding, carry out sofening treatment, but sofening treatment effect is undesirable, and cannot recover after softening, cause intensity in the use procedure of twigs of the chaste tree goods to decline, impact normally uses.
Summary of the invention
The object of this invention is to provide a kind of twigs of the chaste tree softening method, improve the bating effect of the twigs of the chaste tree, and complete laggard row relax in braiding, the intensity of the twigs of the chaste tree can be recovered.
The present invention is achieved through the following technical solutions:
A kind of twigs of the chaste tree softening method, comprises the following steps:
(1), treatment fluid A is prepared, by weight, by 160 parts, water, glycerine 8.6 parts, pine-seed oil 4.5 parts, tributyl phosphate 1.2 parts is heated to 35 DEG C makes it fully mix, and then adds 8.2 parts, urea, 5.2 parts, potassium nitrate, make its abundant mixed dissolution, obtain treatment fluid A;
(2), by the twigs of the chaste tree use treatment fluid immersion treatment 18h at 42 DEG C, then the twigs of the chaste tree are pulled out, weave;
(3), treatment fluid B process, 68 parts, water, polyethylene glycol 4 parts are stirred at 42-45 DEG C, it is made fully to dissolve, then woven twigs of the chaste tree goods are put into and wherein soak, immersion treatment 2h, then add sodium acid carbonate 4.6 parts, sodium salicylate 2.4 parts makes it dissolve, continue to soak 3h, pull out, use clear water to rinse well.
Beneficial effect of the present invention: twigs of the chaste tree softening method provided by the invention is simple, the twigs of the chaste tree can be softened before braiding, reduces the difficulty of braiding, prevents twigs of the chaste tree cracking or fracture in braiding process, improves quality of item; And liquid A and medical liquid B are processed respectively, after liquid A process, twigs of the chaste tree flexibility can be made to increase, when preventing from weaving, the twigs of the chaste tree fracture or ftracture, cause the quality of goods to decline, after braiding completes, use medical liquid B to carry out immersion treatment, the intensity of the twigs of the chaste tree can be made to recover, strengthen its serviceability, make its goods weave lifting more than 30% than direct service time, and in use procedure, goods stability is high, indeformable, and in use procedure, the corrosion resistance of goods is enhanced.Prepared by the present invention can reach more than 10 years rear service time, and can not be out of shape in use procedure.
Detailed description of the invention
A kind of twigs of the chaste tree softening method, comprises the following steps:
(1), treatment fluid A is prepared, by weight, by 160 parts, water, glycerine 8.6 parts, pine-seed oil 4.5 parts, tributyl phosphate 1.2 parts is heated to 35 DEG C makes it fully mix, and then adds 8.2 parts, urea, 5.2 parts, potassium nitrate, make its abundant mixed dissolution, obtain treatment fluid A;
(2), by the twigs of the chaste tree use treatment fluid immersion treatment 18h at 42 DEG C, then the twigs of the chaste tree are pulled out, weave;
(3), treatment fluid B process, 68 parts, water, polyethylene glycol 4 parts are stirred at 42-45 DEG C, it is made fully to dissolve, then woven twigs of the chaste tree goods are put into and wherein soak, immersion treatment 2h, then add sodium acid carbonate 4.6 parts, sodium salicylate 2.4 parts makes it dissolve, continue to soak 3h, pull out, use clear water to rinse well.
Use treatment fluid A of the present invention process, use 700 twigs of the chaste tree of same batch to process, arrange control group, the softening reagent of each group all enters immersion treatment 5h to the twigs of the chaste tree, and result is as following table:
Softening reagent Experiment quantity Ftracture after braiding quantity Number of breaks after braiding Damaged ratio (%)
Softening agent of the present invention 100 3 0 3
Water 100 25 6 31
Glycerine 100 18 3 21
Pine-seed oil 100 15 4 19
73% water+25% glycerine+2% tributyl phosphate 100 9 3 12
65% water+35% glycerine 100 16 4 20
65% water+25% glycerine+10% pine-seed oil 100 15 3 18
Table 1
As shown in Table 1, treatment fluid A of the present invention obviously can promote bating effect relative to conventional softening agent, reduces the damaged ratio of the twigs of the chaste tree in braiding process, improves the quality of finished product.

Claims (1)

1. a twigs of the chaste tree softening method, is characterized in that, comprises the following steps:
(1), treatment fluid A is prepared, by weight, by 160 parts, water, glycerine 8.6 parts, pine-seed oil 4.5 parts, tributyl phosphate 1.2 parts is heated to 35 DEG C makes it fully mix, and then adds 8.2 parts, urea, 5.2 parts, potassium nitrate, make its abundant mixed dissolution, obtain treatment fluid A;
(2), by the twigs of the chaste tree use treatment fluid immersion treatment 18h at 42 DEG C, then the twigs of the chaste tree are pulled out, weave;
(3), treatment fluid B process, 68 parts, water, polyethylene glycol 4 parts are stirred at 42-45 DEG C, it is made fully to dissolve, then woven twigs of the chaste tree goods are put into and wherein soak, immersion treatment 2h, then add sodium acid carbonate 4.6 parts, sodium salicylate 2.4 parts makes it dissolve, continue to soak 3h, pull out, use clear water to rinse well.
CN201510285556.4A 2015-05-29 2015-05-29 Thorn softening method Pending CN104924396A (en)