CN104882646A - 一种废旧锂离子电池的高效安全放电方法 - Google Patents

一种废旧锂离子电池的高效安全放电方法 Download PDF

Info

Publication number
CN104882646A
CN104882646A CN201510293356.3A CN201510293356A CN104882646A CN 104882646 A CN104882646 A CN 104882646A CN 201510293356 A CN201510293356 A CN 201510293356A CN 104882646 A CN104882646 A CN 104882646A
Authority
CN
China
Prior art keywords
lithium ion
ion batteries
salt solution
batteries
waste lithium
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201510293356.3A
Other languages
English (en)
Other versions
CN104882646B (zh
Inventor
宋继顺
许龙
宋大卫
张联齐
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Ant New Energy Technology Tianjin Co ltd
Original Assignee
Tianjin University of Technology
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Tianjin University of Technology filed Critical Tianjin University of Technology
Priority to CN201510293356.3A priority Critical patent/CN104882646B/zh
Publication of CN104882646A publication Critical patent/CN104882646A/zh
Application granted granted Critical
Publication of CN104882646B publication Critical patent/CN104882646B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

一种废旧锂离子电池的高效安全放电方法,步骤如下:1)在饱和盐溶液中加入碱搅拌混合均匀,所述饱和盐溶液中的盐为Na2SO4、K2SO4、NaNO3和KNO3中的一种或两种以上任意比例的混合物,所述碱为Na2CO3、K2CO3、NaOH和KOH中的一种或两种以上任意比例的混合物,饱和盐溶液中加入碱至PH值为10-12,得到混合液;2)将废旧锂离子电池浸泡于上述混合液中进行电解放电,浸泡8-12h后,用钳子手工除去电池的保护电路板,继续浸泡30-40h,使其电解水放电完全;3)将放完电的电池洗净后拆解处理。本发明的优点是:采用该方法处理电池工艺简单、效率高、成本低、更加绿色环保和安全。

Description

一种废旧锂离子电池的高效安全放电方法
技术领域
本发明属于废电池回收处理技术领域,特别是一种废旧锂离子电池的高效安全放电方法
背景技术
随着我国数码产品的广泛普及和电池交通工具的逐步推广,锂离子电池的用量不断增加。与之对应,废旧锂离子电池的产生量也与日俱增。出于环保和资源再利用的角度,废旧锂离子电池的拆解回收势在必行。
对废旧锂离子电池进行拆解回收前首先要对电池进行放电,无论什么样类型尺寸的电池,都要把电量放到安全的程度,否则在后续拆解回收过程中容易发生爆炸,引起事故。而目前在电池拆解回收企业中,对于大尺寸的动力电池,可以采用充放电测试仪逐个放电,而对于小尺寸的数码电池则尚无快速安全简洁的放电方法。为了解决废旧锂离子电池,尤其是小尺寸数码电池的放电问题,本发明设计了一种利用电解水放电的方法,使废旧锂离子电池高效安全地放电完全,避免在后续电池拆解处理过程中发生爆炸。本发明同样适用其他类型的废旧电池放电处理。
发明内容
本发明的目的在于针对上述存在问题,提供一种废旧锂离子电池的高效安全放电方法,采用该方法处理电池具有工艺简单、效率高、成本低、绿色环保、更加安全的优点。
本发明的技术方案:
一种废旧锂离子电池的高效安全放电方法,包括以下步骤:
1)在饱和盐溶液中加入碱搅拌混合均匀,所述饱和盐溶液中的盐为Na2SO4、K2SO4、NaNO3和KNO3中的一种或两种以上任意比例的混合物,所述碱为Na2CO3、K2CO3、NaOH和KOH中的一种或两种以上任意比例的混合物,饱和盐溶液中加入碱至PH值为10-12,得到混合液;
2)将废旧锂离子电池浸泡于上述混合液中进行电解放电,并将容器放在通风良好之处以使产生的氧气和氢气随时排除,浸泡8-12h后,用钳子手工除去电池的保护电路板,继续浸泡30-40h,使其电解水放电完全;
3)将放完电的电池洗净后拆解处理。
本发明的优点是:采用该方法处理电池工艺简单、效率高、成本低、更加绿色环保和安全。
附图说明
图1为实施例1电池在饱和硫酸钠及氢氧化钠的混合液中的电池的电压变化图。
图2为实施例2电池在饱和硫酸钾及氢氧化钠的混合液中的电池的电压变化图。
图3为实施例3电池在饱和硝酸钾及氢氧化钠的混合液中的电池的电压变化图。
具体实施方法
为了使本发明的目的、技术方案及优点更加清楚明白,以下结合附图,对本发明进行进一步详细说明。
实施例1:
一种废旧锂离子电池的高效安全放电方法,包括以下步骤:
1)在饱和硫酸钠溶液中加入氢氧化钠至PH值为10,搅拌混合均匀得到混合液;2)将废旧锂离子电池浸泡于上述混合液中进行电解放电,并将容器放在通风厨中以使产生的氧气和氢气随时排除,浸泡8h后,用钳子手工除去电池的保护电路板,继续浸泡40h,使其电解水放电完全;
3)将放完电的电池洗净后拆解处理。
图1为电池在饱和硫酸钠及氢氧化钠的混合液中的电池的电压变化图,图中表明:一块容量为658.81mAh的废旧锂离子电池完全电解时,电解所得到的氢气的量为0.012295mol。
实施例2:
一种废旧锂离子电池的高效安全放电方法,步骤与实施例1基本相同,不同之处在于:用饱和硫酸钾溶液取代饱和硫酸钠溶液。
图2为电池在饱和硫酸钠及氢氧化钠的混合液中的电池的电压变化图,图中表明:一块容量为221.54mAh的废旧锂离子电池完全电解时,电解所得到的氢气的量为0.00413mol。
实施例3:
一种废旧锂离子电池的高效安全放电方法,步骤与实施例1基本相同,不同之处在于:用饱和硝酸钾溶液取代饱和硫酸钠溶液。
图3为电池在饱和硫酸钠及氢氧化钠的混合液中的电池的电压变化图,图中表明:一块容量为313.33mAh的废旧锂离子电池完全电解时,电解所得到的氢气的量为0.00584mol。

Claims (1)

1.一种废旧锂离子电池的高效安全放电方法,其特征在于包括以下步骤:
1)在饱和盐溶液中加入碱搅拌混合均匀,所述饱和盐溶液中的盐为Na2SO4、K2SO4、NaNO3和KNO3中的一种或两种以上任意比例的混合物,所述碱为Na2CO3、K2CO3、NaOH和KOH中的一种或两种以上任意比例的混合物,饱和盐溶液中加入碱至PH值为10-12,得到混合液;
2)将废旧锂离子电池浸泡于上述混合液中进行电解放电,并将容器放在通风良好之处以使产生的氧气和氢气随时排除,浸泡8-12h后,用钳子手工除去电池的保护电路板,继续浸泡30-40h,使其电解水放电完全;
3)将放完电的电池洗净后拆解处理。
CN201510293356.3A 2015-06-02 2015-06-02 一种废旧锂离子电池的高效安全放电方法 Active CN104882646B (zh)