CN104674602A - Dyeing method for cardboard paper papermaking in surface sizing and dyeing process by paper machine - Google Patents
Dyeing method for cardboard paper papermaking in surface sizing and dyeing process by paper machine Download PDFInfo
- Publication number
- CN104674602A CN104674602A CN201510042874.8A CN201510042874A CN104674602A CN 104674602 A CN104674602 A CN 104674602A CN 201510042874 A CN201510042874 A CN 201510042874A CN 104674602 A CN104674602 A CN 104674602A
- Authority
- CN
- China
- Prior art keywords
- paper
- sizing material
- sizing
- applying glue
- pulp
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
The invention relates to a dyeing method for cardboard paper papermaking in a surface sizing and dyeing process by a paper machine. The method comprises the following steps: (1) prefabricating body paper and a sizing material, wherein the content of solid of the sizing material is 3 to 10 percent, and the viscosity of the sizing material at 70 DEG C is controlled to 5 to 20Pa.s; (2) selecting a model number of a scraper rod, putting the sizing material into a sizing operating trough of the paper machine, wherein the addition amount of the sizing material is 650 to 850L/h, the pressure between the scraper rod and a sizing roller is 50 to 150kpa, and forming a uniform sizing film on a bottom sizing roller; (3) simultaneously adding black dye, red dye and yellow dye into the sizing operating trough, mixing with the sizing material to form a sizing material mixture on the premise of step 2, and laying the surface of the body paper with the sizing material mixture; (4) carrying out the temperature control according to the content of water of a paper web so as to be heated and dried gradually, wherein the surface temperature of the paper is gradually increased from 60 to 100 DEG C until the paper is dried, and the content of the water of the paper web can be within 6 to 10 percent; and (5) coiling finished paper. The method is simple, the single-layer coloring of the paper web is facilitated, and the cupboard paper meeting the requirement can be produced by the single-layer mesh paper machine.
Description
Technical field
The present invention relates to a kind of papermachine surfaces applying glue to dye the colouring method of manufacturing paper with pulp for liner board.
Background technology
Liner board, also known as brown paper, craft paper, is one of main paper kind of carton paper using; Existing liner board adopts Multilayer Network paper machine to produce usually, because liner board need be painted to it according to user's request, and this kind of coloring process is generally directly in process of production be added in the slurry of body paper by dyestuff, directly make through net paper machine, the waste water produced in this production process, waste residue etc. are owing to causing the disposal cost in later stage high containing dyestuff, the consumptive material rate of this kind of mode of production slurry and dyestuff is high simultaneously, the production cost of the enterprise added.
Summary of the invention
A kind of papermachine surfaces applying glue is the object of the present invention is to provide to dye the colouring method of manufacturing paper with pulp for liner board, this simple process, convenient solution paper web individual layer in paper machine is painted, thus makes monolayer net paper machine produce satisfactory liner board, reduces production cost.
Technical program of the present invention lies in: a kind of papermachine surfaces applying glue dyeing is used for the colouring method that boxboard is manufactured paper with pulp, and comprises the following steps:
1) prefabricated body paper and sizing material, the solids content of described sizing material is 3% ~ 10%, and control sizing material is 5 ~ 20Pas the viscosity of 70 DEG C;
2) select scraper model, and add sizing material in the applying glue work nest of paper machine, the interpolation doses of described sizing material is 650 ~ 850L/h, between scraper and application roll pressure be 50 ~ 150kpa, guarantee that bottom application roll forms uniform applying glue film;
3) under the prerequisite of step 2, in applying glue work nest, add black, redness and weld simultaneously make it mix to form size mixture with sizing material, size mixture is executed through scraper and is distributed in body paper surface;
4) carry out temperature according to paper web moisture to control with the oven dry that progressively heats up, the surface temperature of paper, by 60 DEG C ~ 100 DEG C oven dry that progressively heat up, guarantees that the moisture of paper web is 6 ~ 10%;
5) finished paper is batched.
Further, when preparing body paper, in the slurry of body paper, add orchil, its doses is 10 ~ 30L/h; Described sizing material, and by vapour cooking under catalyst action, to be made up after dilution through dissolving of cornstarch or cassava.
Further, the doses of sizing material is 790L/H in step 2, and the pressure between scraper and application roll is 100Kpa.
Further, in step 3, the addition of dyestuff is respectively black 10 ~ 30L/h, yellow 40 ~ 65L/h, red 8 ~ 10L/h.
Further, in step 4, bake out temperature progressively to be heated up oven dry by the heat trnasfer of steam, simultaneously on-line checkingi paper color and adjust chromatic effect and control Substance.
Compared with prior art, the present invention has the following advantages: the papermaking combination utilizing Absorbable organic halogens to control, liquid dyes metering is added in the sizing material of modified surface and forms size mixture, thus size mixture uniform application paper surface completes dyeing, solve paper web individual layer in paper machine painted, and then use monolayer net paper machine to produce the situation of liner board; Save boxboard apparatus for production line, flow process investment cost and production run, maintenance cost; Save water, electricity and gas energy consumption, save dyestuff, reduce production cost, improve economic benefit, reduce environmental pollution.
Detailed description of the invention
For above-mentioned feature and advantage of the present invention can be become apparent, special embodiment below, is described in detail below, but the present invention is not limited to this.
Embodiment one
Papermachine surfaces applying glue dyeing is used for the colouring method that boxboard is manufactured paper with pulp, and comprises the following steps:
1) prefabricated body paper and sizing material, the solids content of described sizing material is 6%, and control sizing material is 15Pas the viscosity of 70 DEG C;
2) select scraper model, and add sizing material in the applying glue work nest of paper machine, the interpolation doses of described sizing material is 790L/h, between scraper and application roll pressure be 100kpa, guarantee that bottom application roll forms uniform applying glue film;
3) under the prerequisite of step 2, in applying glue work nest, add black, redness and weld simultaneously make it mix to form size mixture with sizing material, size mixture is executed through scraper and is distributed in body paper surface;
4) carry out temperature according to paper web moisture to control with the oven dry that progressively heats up, the surface temperature of paper, by 60 DEG C ~ 100 DEG C oven dry that progressively heat up, guarantees that the moisture of paper web is 8%;
5) finished paper is batched.
When preparing body paper, in the slurry of body paper, add orchil, its doses is 20L/h; Described sizing material through dissolving, and forms virgin rubber by vapour cooking by cornstarch or cassava under catalyst action, and the virgin rubber temperature of formation is 115 DEG C, then forms sizing material after dilution, and temperature is at 70 DEG C; Solid content and the viscosity of sizing material can be adjusted according to Production requirement simultaneously.
In step 3, the addition of dyestuff is respectively black 20L/h, yellow 52.5L/h, red 9L/h.
In step 4, oven dry passes in the drying cylinder of paper machine by steam, dried by the heat trnasfer of drying cylinder, steam progressively heats up and controls steam pressure in drying course, simultaneously on-line checkingi paper color and adjust chromatic effect and control Substance, described Substance is the grammes per square metre of one square of rice paper.Such as produce the paper of 80 grammes per square metres, the steam pressure passed in drying cylinder is 80Kpa; 150 grammes per square metre paper, steam pressure 120Kpa.
Embodiment two
Papermachine surfaces applying glue dyeing is used for the colouring method that boxboard is manufactured paper with pulp, and comprises the following steps:
1) prefabricated body paper and sizing material, the solids content of described sizing material is 3%, and control sizing material is 5Pas the viscosity of 70 DEG C;
2) select scraper model, and add sizing material in the applying glue work nest of paper machine, the interpolation doses of described sizing material is 650L/h, between scraper and application roll pressure be 50kpa, guarantee that bottom application roll forms uniform applying glue film;
3) under the prerequisite of step 2, in applying glue work nest, add black, redness and weld simultaneously make it mix to form size mixture with sizing material, size mixture is executed through scraper and is distributed in body paper surface;
4) carry out temperature according to paper web moisture to control with the oven dry that progressively heats up, the surface temperature of paper, by 60 DEG C ~ 100 DEG C oven dry that progressively heat up, guarantees that the moisture of paper web is 6%;
5) finished paper is batched.
When preparing body paper, in the slurry of body paper, add orchil, its doses is 10L/h; Described sizing material, and by vapour cooking under catalyst action, to be made up after dilution through dissolving of cornstarch or cassava.
In step 3, the addition of dyestuff is respectively black 10L/h, yellow 40L/h, red 8L/h.
In step 4, oven dry passes in the drying cylinder of paper machine by steam, dried by the heat trnasfer of drying cylinder, steam progressively heats up and controls steam pressure in drying course, simultaneously on-line checkingi paper color and adjust chromatic effect and control Substance, described Substance is the grammes per square metre of one square of rice paper.Such as produce the paper of 80 grammes per square metres, the steam pressure passed in drying cylinder is 80Kpa; 150 grammes per square metre paper, steam pressure 120Kpa.
Embodiment three
Papermachine surfaces applying glue dyeing is used for the colouring method that boxboard is manufactured paper with pulp, and comprises the following steps:
1) prefabricated body paper and sizing material, the solids content of described sizing material is 10%, and control sizing material is 20Pas the viscosity of 70 DEG C;
2) select scraper model, and add sizing material in the applying glue work nest of paper machine, the interpolation doses of described sizing material is 850L/h, between scraper and application roll pressure be 150kpa, guarantee that bottom application roll forms uniform applying glue film;
3) under the prerequisite of step 2, in applying glue work nest, add black, redness and weld simultaneously make it mix to form size mixture with sizing material, size mixture is executed through scraper and is distributed in body paper surface;
4) carry out temperature according to paper web moisture to control with the oven dry that progressively heats up, the surface temperature of paper, by 60 DEG C ~ 100 DEG C oven dry that progressively heat up, guarantees that the moisture of paper web is 10%;
5) finished paper is batched.
When preparing body paper, in the slurry of body paper, add orchil, its doses is 30L/h; Described sizing material, and by vapour cooking under catalyst action, to be made up after dilution through dissolving of cornstarch or cassava.
In step 3, the addition of dyestuff is respectively black 30L/h, yellow 65L/h, red 10L/h.
In step 4, oven dry passes in the drying cylinder of paper machine by steam, dried by the heat trnasfer of drying cylinder, steam progressively heats up and controls steam pressure in drying course, simultaneously on-line checkingi paper color and adjust chromatic effect and control Substance, described Substance is the grammes per square metre of one square of rice paper.Such as produce the paper of 80 grammes per square metres, the steam pressure passed in drying cylinder is 80Kpa; 150 grammes per square metre paper, steam pressure 120Kpa.
The foregoing is only preferred embodiment of the present invention, for the ordinary skill in the art, according to instruction of the present invention, design the colouring method that multi-form boxboard manufactures paper with pulp and do not need performing creative labour, all equalizations made according to the present patent application the scope of the claims change, revise, replace and modification without departing from the principles and spirit of the present invention, all should belong to covering scope of the present invention.
Claims (5)
1. papermachine surfaces applying glue dyeing is used for the colouring method that liner board is manufactured paper with pulp, and it is characterized in that, comprises the following steps:
1) prefabricated body paper and sizing material, the solids content of described sizing material is 3% ~ 10%, and control sizing material is 5 ~ 20Pas the viscosity of 70 DEG C;
2) select scraper model, and add sizing material in the applying glue work nest of paper machine, the interpolation doses of described sizing material is 650 ~ 850L/h, between scraper and application roll pressure be 50 ~ 150kpa, guarantee that bottom application roll forms uniform applying glue film;
3) under the prerequisite of step 2, in applying glue work nest, add black, redness and weld simultaneously make it mix to form size mixture with sizing material, size mixture is executed through scraper and is distributed in body paper surface;
4) carry out temperature according to paper web moisture to control with the oven dry that progressively heats up, the surface temperature of paper, by 60 DEG C ~ 100 DEG C oven dry that progressively heat up, guarantees that the moisture of paper web is 6 ~ 10%;
5) finished paper is batched.
2. a kind of papermachine surfaces applying glue dyeing according to claim 1 is used for the colouring method that liner board is manufactured paper with pulp, and it is characterized in that, when preparing body paper, in the slurry of body paper, add orchil, its doses is 10 ~ 30L/h; Described sizing material, and by vapour cooking under catalyst action, to be made up after dilution through dissolving of cornstarch or cassava.
3. a kind of papermachine surfaces applying glue dyeing according to claim 1 is used for the colouring method that liner board is manufactured paper with pulp, and it is characterized in that, the doses of sizing material is 790L/H in step 2, and the pressure between scraper and application roll is 100Kpa.
4. a kind of papermachine surfaces applying glue dyeing according to claim 1 is used for the colouring method that liner board is manufactured paper with pulp, and it is characterized in that, in step 3, the addition of dyestuff is respectively black 10 ~ 30L/h, yellow 40 ~ 65L/h, red 8 ~ 10L/h.
5. a kind of papermachine surfaces applying glue dyeing according to claim 1 is used for the colouring method that liner board is manufactured paper with pulp, it is characterized in that, in step 4, bake out temperature progressively to be heated up oven dry by the heat trnasfer of steam, simultaneously on-line checkingi paper color and adjust chromatic effect and control Substance.