CN1045794C - 从高砷铅阳极泥提取金银及有价金属的方法 - Google Patents

从高砷铅阳极泥提取金银及有价金属的方法 Download PDF

Info

Publication number
CN1045794C
CN1045794C CN96112638A CN96112638A CN1045794C CN 1045794 C CN1045794 C CN 1045794C CN 96112638 A CN96112638 A CN 96112638A CN 96112638 A CN96112638 A CN 96112638A CN 1045794 C CN1045794 C CN 1045794C
Authority
CN
China
Prior art keywords
silver
liquid
solid
gold
hour
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN96112638A
Other languages
English (en)
Other versions
CN1177014A (zh
Inventor
杨宗荣
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Kunming Institute of Precious Metals
Original Assignee
Kunming Institute of Precious Metals
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Kunming Institute of Precious Metals filed Critical Kunming Institute of Precious Metals
Priority to CN96112638A priority Critical patent/CN1045794C/zh
Publication of CN1177014A publication Critical patent/CN1177014A/zh
Application granted granted Critical
Publication of CN1045794C publication Critical patent/CN1045794C/zh
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

从高砷铅阳极泥提取金银及有价金属的方法,包括利用NaOH浸出高砷铅阳极泥,并用复合萃取剂从溶液中萃取回收金,其特征是阳极泥在固/液比1∶8~20、温度80~90℃条件下,用100~300g/lNaOH浸出,以除去砷、铅,然后利用已知工艺综合回收金银及其它有价金属。本发明具有除砷彻底、金属回收率高、方法简便、设备简单、无环境污染等优点,适用于从高砷铅阳极泥提取金银及有价金属。

Description

从高砷铅阳极泥提取金银及有价金属的方法
本发明涉及从高砷铅阳极泥中湿法提取金银及有价金属的方法。
高砷物料,特别是高砷阳极泥是有色金属及贵金属的重要原料,脱砷一直是处理该类物料的公认的技术难点。以现有技术(氧化焙烧、加压浸出、细菌浸出、酸性氧化浸出)处理该类物料进行脱砷,往往具有环境污染严重、设备难以解决、周期长、成本高等暂时难以解决的问题。因此,世界上很多国家都在研究如何解决此难题。《贵金属》,1992,13(2),P.30-34报道了一种“高砷低金银的铅阳极泥的高压脱砷”工艺。该文以高砷低金、银铅阳极泥为原料,采用加压浸出脱砷;脱砷渣混酸浸出锑、铋、铜、铅;浸出渣熔炼、电解得成品银;银阳极泥提金。在加压浸出工序中,该文用NaOH浸煮(浓度30~80g/L,以50g/L为佳),浸煮温度110~150℃(150℃为佳),时间2~4小时(2小时为佳),氧压6kg/cm2,总压6.8kg/cm2。该文的砷脱出率在73.4~94.14%,脱锑铋铜铅后产出纯度~99%的金、银合金。该工艺脱砷效果较好,但需高压设备,操作不太安全。
CN1035321A公开了一种用复合萃取剂(包括混合醇加磷酸三丁酯(TBP))生产高纯金的方法,但其仅适用于从溶液中萃取回收金,不能直接应用于高砷固体物料或阳极泥。
本发明的目的在于克服现有技术存在的不足之处,提出一种从高砷铅阳极泥提取金银及有价金属的方法,利用本发明方法,脱砷比较彻底、设备简易、操作方便、成本低、无环境污染、同时又不会带来有价金属损失。
本发明方法包括利用NaOH浸出高砷铅阳极泥,并用CN1035321A中所说的复合萃取剂(混合醇加磷酸三丁酯(TBP))从溶液中萃取回收金;本发明的特征是有下述具体工序:
A、阳极泥在固/液比(即固体/液体比,单位为g/mL或kg/L)=1∶8~20、温度80~90℃条件下,用100~300g/L NaOH搅拌浸出1~6小时,视铅含量不同实验选择NaOH浓度及固/液比,优先推荐的NaOH浓度为180-200g/L,固/液比为1∶10-15;
B、碱浸液冷至室温6~24小时,回收砷精矿结晶;
C、脱砷母液在电压2~3伏、电流密度90~300A/cm2条件下直流电积6~20小时,电积物回收铅精矿;
D、电积母液在80~90℃搅拌下加入石灰(或石灰乳),其量为阳极泥料重的10~30%,作用1~6小时,过滤回收石灰渣,滤液返回工序A;
E、脱砷、铅后的渣控制在365±10℃空气氧化焙烧8~12小时;
F、烧渣磨细后在固/液比1∶4~10,2~3molH2SO4中于80~90℃搅拌浸出1~6小时,浸出液加入NaCl沉淀银,使其呈AgCl,并并入银的提取流程以回收银,母液回收铜;
6、硫酸浸出渣在固/液比1∶4~10,3~5.5mol HCl中于80~90℃搅拌浸出1~6小时,盐酸浸出液搅拌下加1~4倍水1~2小时,滤出沉淀,将沉淀物搅拌下加入到化学计量的稀氨溶液中1~2小时,得Sb2O3
H、水解母液以铁置换回收铋、锑等,置换母液以石灰中和,中和渣送铁厂回收铁,中和母液排放;
l、HCl浸出渣在固/液比1∶4~10,200~300g/LNa2SO3溶液中15~40℃搅拌浸出1~6小时,溶液回收银;
J、一次浸银渣在固/液比1∶4~10、0.2~0.5molH2SO4中加50~100g/L食盐,加金含量5~15倍NaClO3,80~90℃搅拌浸出6~12小时,从浸出剂中用混合醇+TBP复合萃取剂提取纯金;
K、氯化渣重复工序1,两次浸出银溶液搅拌下加水合肼还原得纯银;
L、二次浸银渣送熔炼厂回收锡等有价金属。
在实施本发明方法时,如果原料中砷含量不高,上述工序B可取消;如果原料中金含量甚微,工序J取消,微量金在熔炼厂回收。
同现有技术相比,本发明有如下优点:
1、本发明方法适应范围广,既适合高砷铅阳极泥,也适合低砷铅阳极泥;
2、设备简单,操作方便,设备维修简便,易实现工业化,维修费低;
3、温度较低,能耗较小;
4、试剂消耗少,生产成本低,经济效益好;
5、常压操作,比较安全;
6、提前分离铅,渣量较少,过滤较快,缩短了流程;
7、解决了砷污染问题,且整个流程气氛较好,有利于保护环境。
附图说明:图1是本发明方法的工艺流程图。
实施例1
一种高砷铅阳极泥,其主要成分为(重量%):Au0.0241,Ag8.2,Cu2.79,Fe0.12,As3.24,Sb31.67,Bi0.026,Pb7.38,SiO23.99,Al2O3<1。
取该阳极泥200克,在2L 200g/L NaOH(或相同浓度的回收再生液)中,固/液比1∶10,80℃条件下搅拌浸出2小时,得到浸渣140克。其中各元素脱出率(%):As95.9,Sb24.9,Pb95.33,Cu3.66.浸出液冷却结晶得到下列成分(重量%)的砷精矿:Cu0.33,As13.14,Sb6.97,Pb3.78.母液在3V、100A/cm2条件下直流电积20小时得到下列成分铅精矿(重量%):Cu0.054,As0.74,Pb38.25,Sb28.42.
脱砷、铅渣未进行脱铜,直接进行下一步骤。在固/液比1∶4.5、4.5molHCl中80℃搅拌浸出2小时,得到浸出渣35克,其中各元素的脱出率为(%):Cu99.4,As97.2,Sb91.4,Pb98.6(累计).浸出液经3倍水稀释水解并氨解后得到含锑77.14%的粗锑氧(Sb2O3).HCl浸出渣在固/液比1∶10,250g/L Na2SO4 4溶液中25℃搅拌浸出2小时,溶液回收银。一次浸银渣在固/液比1∶10,0.25MolH2SO4中加50g/L食盐,加4g NaClO3,80-90℃搅拌浸出6小时。浸出液分成三等分,与10ml复合萃取剂(80%混合醇+20%TBP)四份分别接触,萃取及分相3分钟,收集萃取剂,在60-70℃与2克草酸铵水溶液接触1小时,滤出还原的金。后者分别以水和无水乙醇洗净后制得纯金,其纯度为99.9%,回收率96%。浸金渣用前述相同条件再浸一次银。两次浸银液合并,用NaOH处理至NaOH浓度达到0.5Mol,25℃下搅拌加入5.5ml水合肼还原1小时,产出银粉经洗净并以50ml 3Mol HCl浸洗后,产品纯度达到99.9%,回收率达到96%。
本实验中因铋含量低,未单独回收。
实施例2
取如实施例1所说的阳极泥200克,在固/液比1∶10,250g/L NaOH中于85℃搅拌浸出4小时。各元素浸出率为(%):Pb-100,As98,Sb19.73,-24.75.浸出液冷却结晶得到含砷16.02%的砷渣。金和银在脱砷滤液和砷渣中的损失分别在<0.49%,0.02%和<0.02%,<0.0013%.脱砷液经室温3V、100A/cm2条件下直流电积6小时,得到含Sb31.31%、Pb23.02%的锑铅精矿。
脱砷、铅后的渣在375±5℃空气氧化焙烧8小时。烧渣磨细后在固/液比1∶8,3mol H2SO4中于80℃搅拌浸出2小时。浸出液加入5克NaCl沉淀AgCl,并并入银的提取流程以回收银;母液回收铜。硫酸浸出渣再用实施例1的方法脱锑,分离和回收金、银,并分别获得粗锑氧和纯金、纯银。金、银纯度99.9%,回收率96%。
实施例3
一种高砷铅阳极泥,其主要成分为(重量%):Au0.8(g/l),Ag2.91,Cu3.02,As22.93,Sb29.38,Pb6.39,Sn1.19.取该阳极泥200g在固/液比1∶20,200g/L NaOH溶液中,90℃下搅拌浸出6小时。各元素的浸出率为(%):Pb80.8,As94,Sb61.08。银和金富集3倍。以下工序,将富集物按实施例1的方法分离和提纯。副产品砷渣、锑铅渣和粗锑氧。产出银纯度达到99.9%,回收率96%。金的含量很微,未单独回收。

Claims (2)

1、一种从高砷铅阳极泥提取金银及有价金属的方法,包括利用NaOH浸出高砷铅阳极泥,并用复合萃取剂混合醇加磷酸三丁酯从溶液中萃取回收金,本发明的特征是有下述具体工序:
A、阳极泥在固/液比=1∶8~20、温度80~90℃条件下,用100~300g/LNaOH搅拌浸出1~6小时,视铅含量不同实验选择NaOH浓度及固/液比;
B、碱浸液冷至室温6~24小时,回收砷精矿结晶;
C、脱砷母液在电压2~3伏、电流密度90~300A/cm2条件下直流电积6~20小时,电积物回收铅精矿;
D、电积母液在80~90℃搅拌下加入石灰或石灰乳,其量为阳极泥料重的10~30%,作用1~6小时,滤渣回收石灰渣,滤液返回工序A;
E、脱砷、铅后的渣控制在365±10℃空气氧化焙烧8~12小时;
F、烧渣磨细后在固/液比1∶4~10,2~3mol H2SO4中于80~90℃搅拌浸出1~6小时,浸出液加入NaCl沉淀银,使其呈AgCl,并并入银的提取流程以回收银,母液回收铜:
G、硫酸浸出渣在固/液比1∶4~10.3~5.5mol HCl中于80~90℃搅拌浸出1~6小时,盐酸浸出液搅拌下加1~4倍水1~2小时,滤出沉淀,将沉淀物搅拌下加入到化学计量的稀氨溶液中1~2小时,得Sb2O3
H、水解母液以铁置换回收铋、锑,置换母液以石灰中和,中和渣送铁厂回收铁,中和母液排放;
I、HCl浸出渣在固/液比1∶4~10,200~300g/L Na2SO3溶液中15~40℃搅拌浸出1~6小时,溶液回收银;
J、一次浸银渣在固/液比1∶4~10、0.2~0.5mol H2SO4中加50~100g/L食盐,加金含量5~15倍NaClO3,80~90℃搅拌浸出6~12小时,从浸出液中用混合醇+TBP复合萃取剂提取纯金;
K、氯化渣重复工序I,两次浸出银溶液搅拌下加水合肼还原得纯银;
L、二次浸银渣送熔炼厂回收锡等有价金属。
2、按照权利要求1的方法,其特征是所说的浸出剂NaOH浓度为180-200g/L,固/液比为1∶10-15。
CN96112638A 1996-09-16 1996-09-16 从高砷铅阳极泥提取金银及有价金属的方法 Expired - Fee Related CN1045794C (zh)