CN104250492A - Alkali-resistant water-based primer and preparation method thereof - Google Patents

Alkali-resistant water-based primer and preparation method thereof Download PDF

Info

Publication number
CN104250492A
CN104250492A CN201410501637.9A CN201410501637A CN104250492A CN 104250492 A CN104250492 A CN 104250492A CN 201410501637 A CN201410501637 A CN 201410501637A CN 104250492 A CN104250492 A CN 104250492A
Authority
CN
China
Prior art keywords
parts
powder
water
alkali
priming paint
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201410501637.9A
Other languages
Chinese (zh)
Inventor
王建
赵晖
吕万青
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
ANHUI IRON CREATIVE MATERIAL TECHNOLOGY Co Ltd
Original Assignee
ANHUI IRON CREATIVE MATERIAL TECHNOLOGY Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by ANHUI IRON CREATIVE MATERIAL TECHNOLOGY Co Ltd filed Critical ANHUI IRON CREATIVE MATERIAL TECHNOLOGY Co Ltd
Priority to CN201410501637.9A priority Critical patent/CN104250492A/en
Publication of CN104250492A publication Critical patent/CN104250492A/en
Pending legal-status Critical Current

Abstract

The invention belongs to the field of building materials, and discloses an alkali-resistant water-based primer and a preparation method thereof. The water-based primer comprises 15-30 parts of deionized water, 0.5-1.0 part of a wetting dispersant, 0.1-0.3 parts of a defoamer, 5-10 parts of titanium dioxide, 2-5 parts of mica powder, 5-10 parts of talcum powder, 3-5 parts of kaolin, 5-8 parts of wollastonite powder, 15-20 parts of ground calcium carbonate, 30-45 parts of modified acrylic emulsion, 0.1-0.5 parts of a bactericide, 1-2 parts of propylene glycol, 1-2 parts of a coalescing agent, 0.1-0.2 parts of a PH adjuster, and 0.3-1 part of a thickener. In the alkali-resistant water-based primer, the harmful matter content is low; the modified acrylic emulsion is taken as a basic material, so that a coating is endowed with very good basic material adhesive force; and pigment and filler with superfine grain sizes enable a coating film to have better sealing capability and efficiently resist alkalinity of the basic material, and have certain covering power and adjustable colors, so that the consumption of finish paint can be reduced, and the reduction of whole cost for coating is facilitated.

Description

A kind of Alkali-resistant aqueous priming paint and preparation method thereof
?
Technical field
The invention belongs to building material field, relate to a kind of aqueous priming paint, specifically a kind of Alkali-resistant aqueous priming paint and preparation method thereof.
Background technology
Aqueous priming paint is the abbreviation of water-soluble protective primer, for buildings base material wall guard coating.The finish paint of buildings base material metope coating requires to have elegance, pure and fresh decorative effect and nonpoisonous and tasteless environment-friendly function, its performance comprises weathering resistance, resistance to soiling, tint retention, water tolerance, alkali resistance, abrasion resistance, opacifying power, freeze thawing etc., also workability will be considered, shelf characteric and the film forming properties when low-temperature construction and anticorrosion sex change energy simultaneously.In recent years, along with the deterioration of environment, coating and the exterior coating of buildings are except receiving and exposing to the sun and rain, and be also subject to the impact that acid rain and the ultraviolet that causes because of depletion of the ozone layer strengthen, alkali resistance and the closure of these factor External Wall base materials are had higher requirement.The alkali resistance of aqueous priming paint and closure are not very desirable in the market.
Summary of the invention
The object of the invention is to the defect overcoming prior art, a kind of Alkali-resistant aqueous priming paint and preparation method thereof is provided.
Object of the present invention can be achieved through the following technical solutions:
A kind of Alkali-resistant aqueous priming paint, this aqueous priming paint is made up of the raw material of following weight part: deionized water 15-30 part, wetting dispersing agent 0.5-1.0 part, defoamer 0.1-0.3 part, titanium dioxide 5-10 part, mica powder 2-5 part, talcum powder 5-10 part, kaolin 3-5 part, wollastonite powder 5-8 part, water-ground limestone 15-20 part, modified acrylic acid emulsion 30-45 part, sterilant 0.1-0.5 part, propylene glycol 1-2 part, film coalescence aid 1-2 part, PH conditioning agent 0.1-0.2 part, thickening material 0.3-1 part.
Preferably, this aqueous priming paint is made up of the raw material of following weight part: deionized water 20 parts, wetting dispersing agent 0.8 part, defoamer 0.2 part, titanium dioxide 7 parts, mica powder 4 parts, talcum powder 8 parts, kaolin 4 parts, wollastonite powder 6 parts, water-ground limestone 18 parts, modified acrylic acid emulsion 40 parts, 0.3 part, sterilant, propylene glycol 2 parts, film coalescence aid 2 parts, PH conditioning agent 0.2 part, thickening material 0.6 part.
Preferably, described mica powder particle diameter is 1250 orders, and talcum powder particle diameter is 1250 orders, and kaolin particle diameter is 4000 orders, and wollastonite powder particle diameter is 1250 orders, and water-ground limestone particle diameter is 800 orders.
Present invention also offers a kind of method preparing described aqueous priming paint, comprise following concrete steps:
By deionized water, wetting dispersing agent, defoamer mixing, form premixed liquid, stand-by;
Add titanium dioxide, mica powder, talcum powder, kaolin, wollastonite powder, water-ground limestone, after after dispersion, grind to form pigment slurry;
Pigment slurry is joined in modified acrylic acid emulsion, add sterilant, propylene glycol, film coalescence aid, PH conditioning agent, stir;
Add thickening material adjustment viscosity to 85-90KU, obtained finished product coating.
Beneficial effect of the present invention: harmful substance contents of the present invention is low, take modified acrylic acid emulsion as base-material, coating is made to have fabulous base material sticking power, be equipped with ultra-fine grain diameter pigment and filler makes film closed performance better, effective opposing base material alkalescence, and there is certain opacifying power and adjustable color, finish paint consumption can be reduced, contribute to reducing application holistic cost.
Embodiment
For the ease of it will be appreciated by those skilled in the art that the present invention is further illustrated below in conjunction with specific embodiment.The raw material used in the present embodiment all commercially can be bought and obtain.
Embodiment 1
Preparation Alkali-resistant aqueous priming paint: by deionized water 20 parts, wetting dispersing agent 0.8 part and defoamer 0.2 part of Homogeneous phase mixing, form premixed liquid, stand-by;
Add titanium dioxide 7 parts, 1250 order mica powder 4 parts, 1250 order talcum powder 8 parts, 4000 order kaolin 4 parts, 1250 order wollastonite powder 6 parts, 800 order water-ground limestone 18 parts, after after dispersion, grind to form pigment slurry;
Pigment slurry is joined in 40 parts of modified acrylic acid emulsions, add 0.3 part, sterilant, propylene glycol 2 parts, film coalescence aid 2 parts, PH conditioning agent 0.2 part, stir;
Add 0.6 part of thickening material adjustment viscosity to 85KU, obtained finished product coating.
Embodiment 2
Preparation Alkali-resistant aqueous priming paint: by deionized water 30 parts, wetting dispersing agent 0.5 part and defoamer 0.1 part of Homogeneous phase mixing, form premixed liquid, stand-by;
Add titanium dioxide 5 parts, 1250 order mica powder 5 parts, 1250 order talcum powder 10 parts, 4000 order kaolin 5 parts, 1250 order wollastonite powder 8 parts, 800 order water-ground limestone 20 parts, after after dispersion, grind to form pigment slurry;
Pigment slurry is joined in 45 parts of modified acrylic acid emulsions, add 0.5 part, sterilant, propylene glycol 1.5 parts, film coalescence aid 1.5 parts, PH conditioning agent 0.15 part, stir;
Add 1 part of thickening material adjustment viscosity to 90KU, obtained finished product coating.
Embodiment 3
Preparation Alkali-resistant aqueous priming paint: by deionized water 15 parts, wetting dispersing agent 1 part and defoamer 0.3 part of Homogeneous phase mixing, form premixed liquid, stand-by;
Add titanium dioxide 10 parts, 1250 order mica powder 2 parts, 1250 order talcum powder 5 parts, 4000 order kaolin 3 parts, 1250 order wollastonite powder 5 parts, 800 order water-ground limestone 15 parts, after after dispersion, grind to form pigment slurry;
Pigment slurry is joined in 30 parts of modified acrylic acid emulsions, add 0.1 part, sterilant, propylene glycol 1 part, film coalescence aid 1 part, 0.1 part of PH conditioning agent part, stir;
Add 0.3 part of thickening material adjustment viscosity to 88KU, obtained finished product coating.
Above content is only citing made for the present invention and explanation; affiliated those skilled in the art make various amendment to described specific embodiment or supplement or adopt similar mode to substitute; only otherwise depart from invention or surmount this scope as defined in the claims, protection scope of the present invention all should be belonged to.

Claims (4)

1. an Alkali-resistant aqueous priming paint, it is characterized in that, this aqueous priming paint is made up of the raw material of following weight part: deionized water 15-30 part, wetting dispersing agent 0.5-1.0 part, defoamer 0.1-0.3 part, titanium dioxide 5-10 part, mica powder 2-5 part, talcum powder 5-10 part, kaolin 3-5 part, wollastonite powder 5-8 part, water-ground limestone 15-20 part, modified acrylic acid emulsion 30-45 part, sterilant 0.1-0.5 part, propylene glycol 1-2 part, film coalescence aid 1-2 part, PH conditioning agent 0.1-0.2 part, thickening material 0.3-1 part.
2. a kind of Alkali-resistant aqueous priming paint according to claim 1, it is characterized in that, this aqueous priming paint is made up of the raw material of following weight part: deionized water 20 parts, wetting dispersing agent 0.8 part, defoamer 0.2 part, titanium dioxide 7 parts, mica powder 4 parts, talcum powder 8 parts, kaolin 4 parts, wollastonite powder 6 parts, water-ground limestone 18 parts, modified acrylic acid emulsion 40 parts, 0.3 part, sterilant, propylene glycol 2 parts, film coalescence aid 2 parts, PH conditioning agent 0.2 part, thickening material 0.6 part.
3. a kind of Alkali-resistant aqueous priming paint according to claim 1, is characterized in that, described mica powder particle diameter is 1250 orders, and talcum powder particle diameter is 1250 orders, and kaolin particle diameter is 4000 orders, and wollastonite powder particle diameter is 1250 orders, and water-ground limestone particle diameter is 800 orders.
4. prepare a method for aqueous priming paint as claimed in claim 1 or 2, it is characterized in that, comprise following concrete steps:
By deionized water, wetting dispersing agent, defoamer mixing, form premixed liquid, stand-by;
Add titanium dioxide, mica powder, talcum powder, kaolin, wollastonite powder, water-ground limestone, after after dispersion, grind to form pigment slurry;
Pigment slurry is joined in modified acrylic acid emulsion, add sterilant, propylene glycol, film coalescence aid, PH conditioning agent, stir;
Add thickening material adjustment viscosity to 85-90KU, obtained finished product coating.
?
CN201410501637.9A 2014-09-27 2014-09-27 Alkali-resistant water-based primer and preparation method thereof Pending CN104250492A (en)