CN104001892A - 一种中间包氩气流量的调节方法 - Google Patents
一种中间包氩气流量的调节方法 Download PDFInfo
- Publication number
- CN104001892A CN104001892A CN201410258967.XA CN201410258967A CN104001892A CN 104001892 A CN104001892 A CN 104001892A CN 201410258967 A CN201410258967 A CN 201410258967A CN 104001892 A CN104001892 A CN 104001892A
- Authority
- CN
- China
- Prior art keywords
- tundish
- weight
- argon flow
- flow amount
- argon
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
一种中间包氩气流量的调节方法,将原有的中间包上水口固定吹氩气流量更改为根据中间包钢水重量的变化而动态调节吹入氩气流量的方式,来避免中间包钢水液面裸露,保证中间包钢水的洁净度,减轻结晶器内钢水的液位波动,从而提高铸坯质量。与现有的技术相比,本发明的有益效果是:避免了中间包液面的裸露和喷溅,减轻了结晶器液面的波动,从而改善了钢水的洁净度,提高了铸坯质量。
Description
技术领域
本发明涉及连铸技术领域,尤其涉及一种中间包氩气流量的调节方法。
背景技术
连铸中间包作为连铸过程的缓冲环节,能够顺利向结晶器内浇注钢水主要是依靠中间包内钢水自身重力产生的静压力。在更换大罐过程中,前一罐钢水浇注结束至下一罐钢水开浇之前,中间包钢水重量持续下降,从而导致中间包钢水液面高度也持续下降,钢水静压力也持续减小,而中间包上水口氩气流量是设定好的定值,那么在氩气的作用下,钢水向结晶器内的补充不充分,将导致控流装置(滑板或塞棒控流)的开度出现大的波动,导致结晶器液面波动加大。另外,中间包液面的持续降低,在氩气的作用下会导致液面喷溅裸露,这都严重影响钢水洁净度,影响铸坯质量。
发明内容
本发明的目的在于提供一种中间包氩气流量的调节方法,将原有的中间包上水口固定吹氩气流量更改为根据中间包钢水重量的变化而动态调节吹入氩气流量的方式,来避免中间包钢水液面裸露,保证中间包钢水的洁净度,减轻结晶器内钢水的液位波动,从而提高铸坯质量。
为实现上述目的,本发明采用以下技术方案实现:
一种中间包氩气流量的调节方法,通过实际操作得出数据,将得到的拟合方程输入氩气控制箱内的PLC,实现根据中间包重量动态调节中间包上水口氩气吹入量,具体操作步骤如下:
1)在正常浇注情况下,将中间包钢水重量以不超过5吨差值,依次从最大值降低到安全浇注吨位,并在每个重量点处,手动调节氩气流量至中间包液面不裸露、中间包滑板或塞棒等控流装置开度不发生大的波动或起伏为准;
2)将记录的氩气流量值以中间包重量为变量,通过多次实验,将实验结果分阶段拟合,建立分段式的函数方程;
3)将所得到的函数方程编入氩气流量控制箱内的PLC程序内,并将中间包重量实时监测结果信号传入该PLC内,从而实现PLC根据中间包重量的变化动态调节吹入的氩气流量。
与现有的技术相比,本发明的有益效果是:
避免了中间包液面的裸露和喷溅,减轻了结晶器液面的波动,从而改善了钢水的洁净度,提高了铸坯质量。
具体实施方式
下面对本发明的具体实施方式进一步说明:
一种中间包氩气流量的调节方法,通过实际操作得出数据,将得到的拟合方程输入氩气控制箱内的PLC,实现根据中间包重量动态调节中间包上水口氩气吹入量,具体操作步骤如下:
1)在正常浇注情况下,将中间包钢水重量以不超过5吨差值,依次从最大值降低到安全浇注吨位,并在每个重量点处,手动调节氩气流量;从而满足两个条件:一是保证控流装置(滑板或塞棒控流)开度不发生大的波动或者起伏;二是保证中间包液面不裸露,同时记录各重量点所对应的氩气流量值。
2)将记录的氩气流量值以中间包重量为变量,通过多次实验,将实验结果分阶段拟合,建立分段式的函数方程;
3)将所得到的函数方程编入氩气流量控制箱内的PLC程序内,并将中间包重量实时监测结果信号传入该PLC内,从而实现PLC根据中间包重量的变化动态调节吹入的氩气流量。
实施例:
在厚度为230mm板坯连铸机上,中间包满包重量为55吨,以5吨差值降低中间包吨数至25吨,并手动调节氩气流量,所获得与中间包重量对应的氩气流量值如下表所示:
中间包重量(t) | 55 | 50 | 45 | 40 | 35 | 30 | 25 |
氩气流量(NL/min) | 8 | 7.2 | 6.3 | 5 | 3.8 | 3.4 | 2.8 |
通过数据拟合后得到拟合方程式如下:
其中:Q为氩气吹入流量;t为中包实际重量。
将所得到的方程式通过程序编入氩气控制箱内的PLC,将中间包重量信号也接入其中,从而实现根据中间包重量动态调节中间包上水口氩气吹入量。
经实际检查,中间包液面未出现裸露现象,结晶器液面波动大幅减弱,这说明本发明是可行的,可以在板坯连铸中间包上进行使用。
本发明同样适用于任何安装透气上水口的连铸用中间包上使用,原理相同。
Claims (1)
1.一种中间包氩气流量的调节方法,通过实际操作得出数据,将得到的拟合方程输入氩气控制箱内的PLC,实现根据中间包重量动态调节中间包上水口氩气吹入量,其特征在于,具体操作步骤如下:
1)在正常浇注情况下,将中间包钢水重量以不超过5吨差值,依次从最大值降低到安全浇注吨位,并在每个重量点处,手动调节氩气流量至中间包液面不裸露、中间包滑板或塞棒等控流装置开度不发生大的波动或起伏为准;
2)将记录的氩气流量值以中间包重量为变量,通过多次实验,将实验结果分阶段拟合,建立分段式的函数方程;
3)将所得到的函数方程编入氩气流量控制箱内的PLC程序内,并将中间包重量实时监测结果信号传入该PLC内,从而实现PLC根据中间包重量的变化动态调节吹入的氩气流量;所述的氩气流量公式为:
其中:Q为氩气吹入流量;t为中包实际重量。