CN103909022A - 风化型钛铁矿石选钛浮选药剂及浮选钛方法 - Google Patents

风化型钛铁矿石选钛浮选药剂及浮选钛方法 Download PDF

Info

Publication number
CN103909022A
CN103909022A CN201410135811.2A CN201410135811A CN103909022A CN 103909022 A CN103909022 A CN 103909022A CN 201410135811 A CN201410135811 A CN 201410135811A CN 103909022 A CN103909022 A CN 103909022A
Authority
CN
China
Prior art keywords
titanium
minutes
agent
acid
iron ore
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201410135811.2A
Other languages
English (en)
Other versions
CN103909022B (zh
Inventor
张佳楠
孙丰月
王力
张渊
程光渊
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Jilin University
Original Assignee
Jilin University
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Jilin University filed Critical Jilin University
Priority to CN201410135811.2A priority Critical patent/CN103909022B/zh
Publication of CN103909022A publication Critical patent/CN103909022A/zh
Application granted granted Critical
Publication of CN103909022B publication Critical patent/CN103909022B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明涉及一种风化型钛铁矿石选钛浮选药剂及浮选钛的方法,将风化钛铁矿石破碎之100目以下,按质量比加入活化剂,磨矿至-0.074mm;调矿浆浓度至40%;依次加入调整剂、辅助调整剂、捕收剂,辅助捕收剂;粗选、扫选、精选、经一粗一扫二精,获钛精矿品位48%—52%,回收率80%—82%。本发明解决了风化型钛铁矿石的分选问题,使有限的自然资源得已利用。所采用的浮选药剂与现有的浮选药剂不同,无环境污染,药剂价格便宜;浮选工艺流程短,且工艺简单,回收成本低廉,钛的回收率达80%以上。

Description

风化型钛铁矿石选钛浮选药剂及浮选钛方法
技术领域
本发明涉及一种选钛浮选药剂和选钛方法,尤其是从风化型钛铁矿石中选钛的浮选药剂及选钛工艺。
技术背景
钛及化合物合金广泛地用于航天航天军工造船冶金化工机械交通轻工海水淡化环境保护及医疗等领域,属于“战略资源”之一。
地质作用形成的钛铁矿有四种类型:1.与变质基性岩(榴辉岩)有关的金红石矿床;2.与基性岩有关的共伴生型钒钛磁铁矿床(如四川攀枝花 河北大庙)等;3.沉积金红石内陆滨海砂矿;4.风化型殘积钛铁矿床。不同地质作用所形成的矿床矿石组成矿物组合及工业矿物是有区别的:第1.3类型钛矿床矿石组成以金红石为主要工业矿物的组合,第2类型矿床矿石矿物组合是以钛铁矿、钛磁铁矿、磁铁矿等为主要工业矿物,而第4类型钛矿床矿石矿物组合则是以钛赤铁矿、钛磁赤铁矿、磁铁矿等为主要工业矿物,不同组合钛工业矿物的表面化学及物性是有差别的,矿石矿物选别方法也不同。目前针对以金红石和钛铁矿两个组合为主要代表的矿石分选方法和工艺已比较成熟,一般采用浮选法和磁选法,金红石—钛铁矿两组合均可以采用浮选法。已知有TLT(钛酸四异丙酯)药剂浮选法(四川攀枝花)和DYT(钛浮选剂)浮选法(四川攀枝花、河北大庙)。
CN102631980A公开了一种“一种提高钛铁矿选钛回收率的方法”步骤如下:钛铁矿原矿经初次选铁流程选出铁精矿,再通过初次高梯度磁选流程得到初次钛中矿,进行分级细磨流程、二次选铁流程选出次铁精矿,再进入二次高梯度磁选流程得到高品位的二次钛中矿;二次钛中矿进入浮选流程得到钛精矿。
现有的高钛铁矿选钛工艺流程长,回收成本高,回收率低,且不适用于风化型钛铁矿石选钛,致使许多风化型钛铁矿成为呆矿,使有限的自然资源得不到有效利用,浪费了资源。
发明内容
本发明的目的是针对现有技术的不足,提出一种以钛赤铁矿钛磁赤铁矿等为主要工业矿物组合的风化型钛铁矿石选钛浮选药剂;
本发明的另一目的是提出一种以钛赤铁矿钛磁赤铁矿等为主要工业矿物组合的风化型钛铁矿石选钛的浮选方法。
本发明的目的是通过以下技术方案实现的:
针对风化作用所形成的钛铁矿石矿物组合及工业矿物特征性质等因素,采用先将钛矿物活化,加酸调整,再进行浮选。
浮选药剂按质量比:
所述的活化剂为草酸,调整剂为盐酸或硝酸,辅助调整剂为Na2SiO4,捕收剂为脂酸,辅助捕收剂为2号油。
所述的脂酸为油脂酸、硬脂酸或软脂酸中的一种。
风化型钛铁矿石浮选钛方法,包括以下步骤:
a、将风化钛铁矿石破碎之100目以下,按质量比加入160g/t~400g/t活化剂,磨矿至-0.074mm;
b、调矿浆浓度至40%;
c、依次加入调整剂2500g/t~4500g/t,辅助调整剂800g/t~4000g/t,搅拌2分钟;
d、再依次加入捕收剂2500g/t~4800g/t,辅助捕收剂60g/t~180g/t;
e、粗选8—10分钟,扫选8—10分钟,精选3—6分钟,再次精选2—5分钟。
经一粗一扫二精,获钛精矿品位48%—52%,回收率80%—82%。
有益效果:本发明解决了风化型钛铁矿石的分选问题,使有限的自然资源得已利用。所采用的浮选药剂与现有的浮选药剂不同,无环境污染,药剂价格便宜;浮选工艺流程短,且工艺简单,回收成本低廉,钛的回收率达80%以上。
附图说明
附图为风化型钛铁矿石浮选钛方法流程图
具体实施方式
下面结合实施例对本发明作进一步的详细说明:
浮选药剂按质量比:
所述的活化剂为草酸,调整剂为盐酸或硝酸,辅助调整剂为Na2SiO4,捕收剂为脂酸,辅助捕收剂为2号油。
所述的脂酸为油脂酸、硬脂酸或软脂酸中的一种。
风化型钛铁矿石浮选钛的方法,包括以下步骤:
a、将风化钛铁矿石破碎之100目以下,按质量比加入160g/t~400g/t活化剂,磨矿至-0.074mm;
b、调矿浆浓度至40%;
c、依次加入调整剂2500g/t~4500g/t,辅助调整剂800g/t~4000g/t,搅拌2分钟;
d、再依次加入捕收剂2500g/t~4800g/t,辅助捕收剂60g/t~180g/t;
e、粗选8—10分钟,扫选8—10分钟,精选3—6分钟,再次精选2—5分钟。
实施例1
取云南某风化钛铁矿石1000g,加草酸0.2g磨矿至-0.074mm,调矿浆浓度至40%,搅拌,依次加H2sO42g,Na2siO41.8g,2分钟后加入2号油0.08g,油脂酸2.4g,粗选8分钟,扫选8分钟,第一次精选6分钟,再次精选3分钟,经一粗一扫二精,获钛精矿品位48.96%,回收率81.98%。
实施例2
取云南某风化钛铁矿石重砂1000g,加草酸0.3g,磨矿至-0.074mm,调矿浆浓度至30%,搅拌,依次加入H2SO42.5g,Na2SiO42.6g,硬脂酸2.8g,2号油0.09g,粗选10分钟,扫选8分钟,精选2次每次4分钟,经一粗一扫二精,获得钛精矿51.8%,回收率80.6%。
实施例3
取内蒙古某风化型钛铁矿石1000g,加草酸0.25g,磨矿至0.074mm,调矿浆浓度至40%,搅拌,依次加入H2SO41.6g,Na2SiO42.7g,软脂酸2.9g,2号油0.6g,粗选9分钟,扫选8分钟,2次精选每次5分钟,经一粗一扫二精,获得钛精矿品位49.6%,回收率80.78%。
实施例4
取四川某风化钛铁矿石1000g,加草酸0.15g,磨矿至0.074mm,调矿浆浓度至40%,依次加入Ha2SO41.5g,Na2SiO42.0g,油脂酸2.95g,2号油0.07g,,粗选10分钟,扫选10分钟,第一次精选6分钟,再次精选3分钟,经一粗一扫二精,获钛精矿品位51.56%,回收率80.18%。
实施例5
5.取云南某风化型钛铁矿石1000g,加草酸0.2g,Na2SiO22.6g,磨矿至0.074mm,调矿浆浓度至30%,依次加入Ha2SO41.58g,软脂酸3.0g,2号油0.05g,粗选8分钟,扫选10分钟,精选2次每次5分钟,经一粗一扫二精,获钛精矿品位49.8%,回收率80.98。

Claims (4)

1.一种风化型钛铁矿石选钛浮选药剂,其特征在于,按质量比: 
2.按照权利要求1所述的风化型钛铁矿石选钛浮选药剂,其特征在于,活化剂为草酸,调整剂为盐酸或硝酸,辅助调整剂为Na2SiO4,捕收剂为脂酸,辅助捕收剂为2号油。 
3.按照权利要求2所述的风化型钛铁矿石选钛浮选药剂,其特征在于,所述的脂酸为油脂酸、硬脂酸或软脂酸中的一种。 
4.一种风化型钛铁矿石选钛方法,其特征在于,包括以下步骤: 
a、将风化钛铁矿石破碎之100目以下,按质量比加入160g/t~400g/t活化剂,磨矿至-0.074mm; 
b、调矿浆浓度至40%; 
c、依次加入调整剂2500g/t~4500g/t,辅助调整剂1800g/t~4000g/t,搅拌2分钟; 
d、再依次加入捕收剂2500g/t~4800g/t,辅助捕收剂60g/t~180g/t; 
e、粗选8—10分钟,扫选8—10分钟,精选3—6分钟,再次精选2—5分钟。 
经一粗一扫二精,获钛精矿品位48%—52%,回收率80%—82%。 
CN201410135811.2A 2014-04-07 2014-04-07 风化型钛铁矿石选钛浮选药剂及浮选钛方法 Expired - Fee Related CN103909022B (zh)