CN103627385B - 一种在酸化液中应用的耐温型铁离子稳定剂 - Google Patents

一种在酸化液中应用的耐温型铁离子稳定剂 Download PDF

Info

Publication number
CN103627385B
CN103627385B CN201310609305.8A CN201310609305A CN103627385B CN 103627385 B CN103627385 B CN 103627385B CN 201310609305 A CN201310609305 A CN 201310609305A CN 103627385 B CN103627385 B CN 103627385B
Authority
CN
China
Prior art keywords
acid
sodium
heat
resistance type
different
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN201310609305.8A
Other languages
English (en)
Other versions
CN103627385A (zh
Inventor
钱程
钱桥胜
张秀霞
谢名璐
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN201310609305.8A priority Critical patent/CN103627385B/zh
Publication of CN103627385A publication Critical patent/CN103627385A/zh
Application granted granted Critical
Publication of CN103627385B publication Critical patent/CN103627385B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种在酸化液中应用的耐温型铁离子稳定剂,包括以下组分:异Vc酸和/或异Vc钠、柠檬酸、盐酸羟胺或二乙烯三胺五乙酸钠。克服了不耐高温、络合铁离子浓度有限的缺陷。

Description

一种在酸化液中应用的耐温型铁离子稳定剂
技术领域
本发明涉及技术领域,特别是涉及一种在酸化液中应用的耐温型铁离子稳定剂。
背景技术
目前,国内外油田油水井酸化处理,是利用酸液的化学溶蚀作用,溶解地层中的岩石矿物、堵塞物,疏通地层孔喉通道,以恢复和提高地层的渗透率,减少油流入井阻力或注水阻力,从而达到油井增产、水井增注的目的。在油水井酸化作业过程中,高浓度的酸溶液在搅拌和泵送过程中会溶解管线和设备表面的铁化合物,进入地层后又会侵蚀岩石中的铁质矿物和粘土矿物,尽管使用了缓蚀剂,但也会溶蚀部分铁。这些溶解铁在溶液中一般以Fe2+和Fe3+状态存在。随着酸液与地层岩石的持续反应,酸液的有效浓度逐渐减低,pH值升高。当酸液pH值上升到2.2(Fe3+的浓度为0.01mol/L)时,就开始产生Fe(OH)3沉淀;当酸液pH值继续上升到3.2时,所有溶解的Fe3+沉淀完全;当酸液pH值继续上升到7.7时,Fe2+同样会产生Fe(OH)2沉淀,但由于酸液的pH值均小于6,因此酸化施工中不考虑Fe(OH)2沉淀。Fe(OH)3沉淀一经形成,就可能堵塞地层孔隙及油气渗透通道,进而降低酸化处理效果和油气产能。为了防止酸液变成残酸时产生铁沉淀,在酸化技术中常采用在酸液中加入铁离子稳定剂来防止酸液变成残酸时生成凝胶状的氢氧化铁沉淀,防止其对油气层的损害,从而提高酸化处理效果。
铁离子稳定剂能从络合、还原、分散三个方面阻止Fe3+的再沉淀。铁离子稳定剂的主要成份是有机酸及其盐。主要用于油气井酸化作业,具有阻止Fe3+沉淀伤害地层的作用。油田目前应用的只是络合物且耐温不高,在150℃以上时作用减小甚至丧失稳定作用,或络合铁离子浓度有限,满足不了需要,因此需要一种耐温型铁离子稳定剂来改善这种不耐高温、络合铁离子浓度有限的问题。
发明内容
本发明的目的就是针对上述存在的缺陷而提供一种在酸化液中应用的耐温型铁离子稳定剂。包括络合剂,PH值调节剂,还原剂等几种组合体,克服了不耐高温、络合铁离子浓度有限的缺陷。
本发明的一种在酸化液中应用的耐温型铁离子稳定剂技术方案为,包括以下组分:异Vc酸和/或异Vc钠、柠檬酸、盐酸羟胺或二乙烯三胺五乙酸钠。
为固体制剂或液体制剂。
固体制剂包括按重量百分比的以下组分:
纯度为99%的异Vc酸36-46%
纯度为99%的柠檬酸48-57%
纯度为97%的盐酸羟胺3-8%。
固体制剂包括按重量百分比的以下组分:
纯度为99%的异Vc钠32-38%
纯度为99%的柠檬酸56-58%
纯度为97%的盐酸羟胺3-10%。
液体制剂包括按重量百分比的以下组分:
异Vc钠5-9%
柠檬酸8-15%
二乙烯三胺五乙酸钠5-12%
水余量。
液体制剂包括按重量百分比的以下组分:
异Vc钠6.0-10%
柠檬酸7-14%
二乙烯三胺五乙酸钠5-12%
水余量。
本发明的有益效果为:本发明的一种在酸化液中应用的耐温型铁离子稳定剂,用于油气井酸化作业,具有阻止Fe3+沉淀伤害地层的作用。耐高温,在150℃以上时作用仍然能起到作用,络合铁离子浓度高,能充分满足生产需要,是一种有效的耐温型铁离子稳定剂,克服了不耐高温、络合铁离子浓度有限的缺陷。
具体实施方式:
为了更好地理解本发明,下面用具体实例来详细说明本发明的技术方案,但是本发明并不局限于此。
实施例1
固体制剂A包括按重量百分比的以下组分:
纯度为99%的异Vc酸40%
纯度为99%的柠檬酸55%
纯度为97%的盐酸羟胺5%
将该制剂A投入实际生产使用,在120℃,15MPa的情况下,24h后,酸液中未见铁离子沉绽.
将该制剂A投入实际生产使用,在155℃,15MPa的情况下,24h后,酸液中未见铁离子沉绽。
实施例2
固体制剂B包括按重量百分比的以下组分:
纯度为99%的异Vc钠32%
纯度为99%的柠檬酸58%
纯度为97%的盐酸羟胺10%
将该制剂A投入实际生产使用,在120℃,15MPa的情况下,24h后,酸液中未见铁离子沉淀。
将该制剂A投入实际生产使用,在155℃,15MPa的情况下,24h后,酸液中未见铁离子沉淀。
实施例3
固体制剂C包括按重量百分比的以下组分:
纯度为99%的异Vc钠36%
纯度为99%的柠檬酸56%
纯度为97%的盐酸羟胺8%
将该制剂A投入实际生产使用,在120℃,15MPa的情况下,24h后,酸液中未见铁离子沉淀。
将该制剂A投入实际生产使用,在155℃,15MPa的情况下,24h后,酸液中未见铁离子沉淀。
实施例4
液体制剂D包括按重量百分比的以下组分:
异Vc钠7%
柠檬酸12%
二乙烯三胺五乙酸钠5%
水余量
将该制剂A投入实际生产使用,在120℃,15MPa的情况下,24h后,酸液中未见铁离子沉淀。
将该制剂A投入实际生产使用,在155℃,15MPa的情况下,24h后,酸液中未见铁离子沉淀。
实施例5
液体制剂E包括按重量百分比的以下组分:
异Vc钠8%
柠檬酸11%
二乙烯三胺五乙酸钠8%
水余量
实施例6
液体制剂F包括按重量百分比的以下组分:
异Vc钠10%
柠檬酸8%
二乙烯三胺五乙酸钠12%
水余量
将该制剂A投入实际生产使用,在120℃,15MPa的情况下,24h后,酸液中未见铁离子沉淀。
将该制剂A投入实际生产使用,在155℃,15MPa的情况下,24h后,酸液中未见铁离子沉淀。

Claims (1)

1.一种在酸化液中应用的耐温型铁离子稳定剂,其特征在于,该稳定剂为液体制剂,液体制剂包括按重量百分比的以下组分:
异Vc钠6-9%
柠檬酸8-14%
二乙烯三胺五乙酸钠5-12%
水余量。
CN201310609305.8A 2013-11-27 2013-11-27 一种在酸化液中应用的耐温型铁离子稳定剂 Expired - Fee Related CN103627385B (zh)