CN103553349A - Manufacturing method of glass touchpad with different hand feel - Google Patents
Manufacturing method of glass touchpad with different hand feel Download PDFInfo
- Publication number
- CN103553349A CN103553349A CN201310473725.8A CN201310473725A CN103553349A CN 103553349 A CN103553349 A CN 103553349A CN 201310473725 A CN201310473725 A CN 201310473725A CN 103553349 A CN103553349 A CN 103553349A
- Authority
- CN
- China
- Prior art keywords
- glass
- face glass
- manufacture method
- touch panels
- etching machine
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention discloses a manufacturing method of a glass touchpad with different hand feel. The method is as below: first dividing an alternative glass panel into sub glass plates in multiple dimensions and suitable for arrangement on consumer electronic products, then conducting washing quality inspection and selecting glass panels with clean surface and no stain for standby; applying the four edges of the glass panel with adhesive tapes, then fixing the glass panel in a PVC sheet material, placing the glass panel in a first etching machine, adding sulfuric acid for a first etching, adding a proper amount of sulfuric acid with concentration of 2%-5% for a first pickling, carrying out a second washing quality inspection, conducting a secondary etching by using a mixed solution of hydrofluoric acid and ammonium fluoride, and finally carrying out a second pickling and washing quality inspection and drying to obtain the touchpad ready for usage. The method can produce glass touchpad with different hand feel, and breaks through the imprisonment that a single handle electronic product cannot realize customization.
Description
Technical field
The present invention relates to a kind of glass touch panel, relate in particular to a kind of manufacture method with different feel glass touch panels.
Background technology
Along with the advanced IT application of modern society, glass touch panel is widely used in electronics every field, and glass touch-control electronic product, still in single feel state, cannot reach customized at present.
Summary of the invention
In order to solve the technical problem existing in background technology, the present invention proposes a kind of manufacture method with different feel glass touch panels, make the diversification of product sense of touch, realize customizedly, satisfy the demands of consumers.
The invention provides a kind of manufacture method with different feel glass touch panels, comprise the following steps:
S1, select base material: alternative face glass is washed to product examine, select surperficial cleaning, spotless face glass standby;
S2, an etching: by four edge adhesive tape gluings of face glass, then be fixed in PVC sheet material, be placed in the first etching machine, in the first etching machine, add the first solution, start and heat the first etching machine and continued for the first period, to allow described the first solution diffusion in described face glass;
S3, a pickling: add appropriate rare sulfuric acid of converting to carry out a pickling, the impurity on face glass surface is departed from;
S4, once wash product examine: the face glass after a pickling is washed to product examine, clean up the impurity that remains in face glass surface after a pickling completes;
S5, second etch: face glass is placed in the second etching machine, in the second etching machine, adds the second solution, start and heat the second etching machine and continued for the second period, to allow described the second solution diffusion in described face glass;
S6, white picking: add appropriate rare sulfuric acid of converting to carry out white picking, the impurity on face glass surface is departed from;
S7, secondary washing product examine: the face glass after white picking is washed to product examine, clean up the impurity that remains in face glass surface after white picking completes.
Further, described step S1 also comprises:
S101, the face glass after selecting is divided into a plurality of sizes is suitable for being arranged on the sub-sheet glass in consumer.
Preferably, described the first solution is sulfuric acid.
Preferably, described the first etching machine is heated to 10-30 degree Celsius.
Preferably, described the first period is 5-30 minute.
Further, described the second solution at least comprises hydrofluoric acid and Neutral ammonium fluoride.
Preferably, described the second etching machine is heated to 10-40 degree Celsius.
Preferably, described the second period is 5-30 minute.
Preferably, the rare sulfuric acid concentration of converting adding in a pickling and white picking is 2%-5%.
The manufacture method described in provided by the invention with different feel glass touch panels carries out respectively with sulfuric acid and hydrofluoric acid and Neutral ammonium fluoride the glass touch panel that etching produces different senses of touch by least one surface at face glass, has broken through single feel electronic product and cannot reach customized confinement.
Accompanying drawing explanation
Fig. 1 is a kind of process flow sheet with the manufacture method of different feel glass touch panels provided by the invention.
Embodiment
Below in conjunction with accompanying drawing, embodiments of the invention are described in detail.
Refer to Fig. 1, the invention provides a kind of manufacture method with different feel glass touch panels, comprise the following steps:
S1, select base material: alternative face glass is divided into a plurality of sizes and is suitable for being arranged on the sub-sheet glass in consumer, then wash product examine, select surperficial cleaning, spotless face glass standby;
S2, an etching: by four edge adhesive tape gluings of face glass, then be fixed in PVC sheet material, be placed in the first etching machine, in the first etching machine, add sulfuric acid, start and heat the first etching machine to 10-30 degree Celsius, continue 5-30 minute, to allow described sulfuric acid to be diffused in described face glass;
S3, a pickling: adding appropriate concentration is that the sulfuric acid of 2%-5% carries out a pickling, and the impurity on face glass surface is departed from;
S4, once wash product examine: the face glass after a pickling is washed to product examine, clean up the impurity that remains in face glass surface after a pickling completes;
S5, second etch: face glass is placed in the second etching machine, toward the mixed solution that adds hydrofluoric acid and Neutral ammonium fluoride in the second etching machine, start and heat the second etching machine to 10-40 degree Celsius, continue 5-30 minute, to allow described the second solution diffusion in described face glass;
S6, white picking: adding appropriate concentration is that the sulfuric acid of 2%-5% carries out white picking, and the impurity on face glass surface is departed from;
S7, secondary washing product examine: the face glass after white picking is washed to product examine, clean up the impurity that remains in face glass surface after white picking completes.
The above-mentioned manufacture method with different feel glass touch panels carries out respectively with sulfuric acid and hydrofluoric acid and Neutral ammonium fluoride the glass touch panel that etching produces different senses of touch by least one surface at face glass, has broken through single feel electronic product and cannot reach customized confinement.
The above; it is only preferably embodiment of the present invention; but protection scope of the present invention is not limited to this; anyly be familiar with those skilled in the art in the technical scope that the present invention discloses; according to technical scheme of the present invention and inventive concept thereof, be equal to replacement or changed, within all should being encompassed in protection scope of the present invention.
Claims (9)
1. a manufacture method with different feel glass touch panels, is characterized in that, comprises the following steps:
S1, select base material: alternative face glass is washed to product examine, select surperficial cleaning, spotless face glass standby;
S2, an etching: by four edge adhesive tape gluings of face glass, then be fixed in PVC sheet material, be placed in the first etching machine, in the first etching machine, add the first solution, start and heat the first etching machine and continued for the first period, to allow described the first solution diffusion in described face glass;
S3, a pickling: add appropriate rare sulfuric acid of converting to carry out a pickling, the impurity on face glass surface is departed from;
S4, once wash product examine: the face glass after a pickling is washed to product examine, clean up the impurity that remains in face glass surface after a pickling completes;
S5, second etch: face glass is placed in the second etching machine, in the second etching machine, adds the second solution, start and heat the second etching machine and continued for the second period, to allow described the second solution diffusion in described face glass;
S6, white picking: add appropriate rare sulfuric acid of converting to carry out white picking, the impurity on face glass surface is departed from;
S7, secondary washing product examine: the face glass after white picking is washed to product examine, clean up the impurity that remains in face glass surface after white picking completes.
2. a kind of manufacture method with different feel glass touch panels according to claim 1, is characterized in that, described step S1 also comprises:
S101, the face glass after selecting is divided into a plurality of sizes is suitable for being arranged on the sub-sheet glass in consumer.
3. a kind of manufacture method with different feel glass touch panels according to claim 1, is characterized in that, described the first solution is sulfuric acid.
4. a kind of manufacture method with different feel glass touch panels according to claim 1, is characterized in that, described the first etching machine is heated to 10-30 degree Celsius.
5. a kind of manufacture method with different feel glass touch panels according to claim 1, is characterized in that, described the first period is 5-30 minute.
6. a kind of manufacture method with different feel glass touch panels according to claim 1, is characterized in that, described the second solution at least comprises hydrofluoric acid and Neutral ammonium fluoride.
7. a kind of manufacture method with different feel glass touch panels according to claim 1, is characterized in that, described the second etching machine is heated to 10-40 degree Celsius.
8. a kind of manufacture method with different feel glass touch panels according to claim 1, is characterized in that, described the second period is 5-30 minute.
9. a kind of manufacture method with different feel glass touch panels according to claim 1, is characterized in that, the rare sulfuric acid concentration of converting adding in a pickling and white picking is 2%-5%.