CN102320805B - 具有防火和保温功能的吸音板及其加工方法 - Google Patents

具有防火和保温功能的吸音板及其加工方法 Download PDF

Info

Publication number
CN102320805B
CN102320805B CN 201110168445 CN201110168445A CN102320805B CN 102320805 B CN102320805 B CN 102320805B CN 201110168445 CN201110168445 CN 201110168445 CN 201110168445 A CN201110168445 A CN 201110168445A CN 102320805 B CN102320805 B CN 102320805B
Authority
CN
China
Prior art keywords
parts
weight part
zinc borate
xps
water glass
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN 201110168445
Other languages
English (en)
Other versions
CN102320805A (zh
Inventor
苏建丽
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nantong Huahong chemical equipment manufacturing and installation Co., Ltd.
Original Assignee
Qingdao Wenchuang Technology Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Qingdao Wenchuang Technology Co Ltd filed Critical Qingdao Wenchuang Technology Co Ltd
Priority to CN 201110168445 priority Critical patent/CN102320805B/zh
Publication of CN102320805A publication Critical patent/CN102320805A/zh
Application granted granted Critical
Publication of CN102320805B publication Critical patent/CN102320805B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明涉及一种具有防火和保温功能的吸音板,其特征在于,包括以下重量份的组份:膨胀珍珠岩30-50份,水玻璃30-50份,玻璃纤维5-10份,硼酸锌5-10份 石灰粉 10-20份;通过对底板、聚苯乙烯板和顶层的分别加工加压得到的保温板,本发明通过在两层混合料浆的中间夹设有聚苯乙烯板,在防火和吸音的同时,保温效果也明显提高。

Description

具有防火和保温功能的吸音板及其加工方法
技术领域
本发明涉及具有防火和保温功能的吸音板,属于建筑材料领域。
背景技术
目前,用膨胀珍珠岩制造吸声板,主要方法有水泥作凝胶,加
适量促凝材料,经成型、养护、自然干燥而成;有用水玻璃作凝胶
材料、用氟硅酸纳促凝,经成型、自然干燥或用封闭室内烘干调解放气孔干燥;也有用有机胶作凝胶材料的,用类似水玻璃作凝胶材料的方法制造。
通过上述方法加工而制备的板材防火性能差、隔音效果差和不具备保温的功能,而且成本高。
发明内容
本发明的目的是提供一种具有防火和保温功能的吸音板,以解决现有技术存在的防火性能差、隔音效果差和不具备保温的功能,而且成本高的问题。本发明的技术方案是:一种具有防火和保温功能的吸音板,其特征在于,包括以下重量份的组份:膨胀珍珠岩30-50份,水玻璃30-50份,玻璃纤维5-10份, 硼酸锌5-10份  石灰粉  10-20份 。  
优选的,包括以下重量份的组份:膨胀珍珠岩 40份,水玻璃  40份,玻璃纤维 8份,   硼酸锌8份  石灰粉  15份。
所述的具有防火和保温功能的吸音板的加工方法,其特征在于,包括以下步骤:
(1)选取的同一色度的膨胀珍珠岩用球磨机进行球磨,并使其颗粒的粒径为0.1-0.19mm,或者为1.1-3mm;
(2)将球磨完毕1/2重量份的膨胀珍珠岩与1/2重量份的石灰粉进行充分混合,并搅拌均匀;
(3)依次分别加入均为1/2重量份的水玻璃、玻璃纤维和硼酸锌;
(4)将上述混合料浆置入模具中并在压力机中进行轻压,使料浆不流动保持稳定即可,所需压力为20Mpa,得到底板;
(5) 在底板上放置一层聚苯乙烯板;
(6)将剩余的珍珠岩、水玻璃、玻璃纤维和硼酸锌进行充分混合,置于聚苯乙烯板的上面,得到顶层;
(6)将底板、聚苯乙烯板和顶层放入压力机中进行压制成坯,压强保持在50-60Mpa;
(7)将成型坯在带有出气孔的烘干室内进行烘干,使烘干室内的温度保持在50-100℃,持续15小时,即得。
本发明通过在两层混合料浆的中间夹设有聚苯乙烯板,在防火和吸音的同时,保温效果也明显提高。
具体实施方式
实施例1: 一种具有防火和保温功能的吸音板,:包括以下重量份的组份:膨胀珍珠岩30份,水玻璃30份,玻璃纤维5份, 硼酸锌5份  石灰粉  10份 。  
所述的具有防火和保温功能的吸音板的加工方法,包括以下步骤:
(1)选取的同一色度的膨胀珍珠岩用球磨机进行球磨,并使其颗粒的粒径为0.1-0.19mm,或者为1.1-3mm; 经过从现有技术中选取的大量的实验证明,当珍珠岩颗粒粒径处于此范围之内时,珍珠岩与其它组份的混合可以取得最佳吸音粒径。
(2)将球磨完毕1/2重量份的膨胀珍珠岩与1/2重量份的石灰粉进行充分混合,并搅拌均匀;
(3)依次分别加入均为1/2重量份的水玻璃、玻璃纤维和硼酸锌;
(4)将上述混合料浆置入模具中并在压力机中进行轻压,使料浆不流动保持稳定即可,所需压力为20Mpa,得到底板;
(5) 在底板上放置一层聚苯乙烯板;
(6)将剩余的珍珠岩、水玻璃、玻璃纤维和硼酸锌进行充分混合,置于聚苯乙烯板的上面,得到顶层;
(6)将底板、聚苯乙烯板和顶层放入压力机中进行压制成坯,压强保持在50-60Mpa;
(7)将成型坯在带有出气孔的烘干室内进行烘干,使烘干室内的温度保持在50℃,持续15小时,即得。
实施例2:
一种具有防火和保温功能的吸音板,包括以下重量份的组份:膨胀珍珠岩 40份,水玻璃  40份,玻璃纤维 8份,   硼酸锌8份  石灰粉  15份。
所述的具有防火和保温功能的吸音板的加工方法,包括以下步骤:
(1)选取的同一色度的膨胀珍珠岩用球磨机进行球磨,并使其颗粒的粒径为0.1-0.19mm,或者为1.1-3mm; 
(2)将球磨完毕1/2重量份的膨胀珍珠岩与1/2重量份的石灰粉进行充分混合,并搅拌均匀;
(3)依次分别加入均为1/2重量份的水玻璃、玻璃纤维和硼酸锌;
(4)将上述混合料浆置入模具中并在压力机中进行轻压,使料浆不流动保持稳定即可,所需压力为20Mpa,得到底板;
(5) 在底板上放置一层聚苯乙烯板;
(6)将剩余的珍珠岩、水玻璃、玻璃纤维和硼酸锌进行充分混合,置于聚苯乙烯板的上面,得到顶层;
(6)将底板、聚苯乙烯板和顶层放入压力机中进行压制成坯,压强保持在50-60Mpa;
(7)将成型坯在带有出气孔的烘干室内进行烘干,使烘干室内的温度保持在80℃,持续15小时,即得。
实施例3:
一种具有防火和保温功能的吸音板,其特征在于,包括以下重量份的组份:膨胀珍珠岩50份,水玻璃50份,玻璃纤维10份, 硼酸锌10份  石灰粉 20份 。  
所述的具有防火和保温功能的吸音板的加工方法,其特征在于,包括以下步骤:
(1)选取的同一色度的膨胀珍珠岩用球磨机进行球磨,并使其颗粒的粒径为0.1-0.19mm,或者为1.1-3mm;
(2)将球磨完毕1/2重量份的膨胀珍珠岩与1/2重量份的石灰粉进行充分混合,并搅拌均匀;
(3)依次分别加入均为1/2重量份的水玻璃、玻璃纤维和硼酸锌;
(4)将上述混合料浆置入模具中并在压力机中进行轻压,使料浆不流动保持稳定即可,所需压力为20Mpa,得到底板;
(5) 在底板上放置一层聚苯乙烯板;
(6)将剩余的珍珠岩、水玻璃、玻璃纤维和硼酸锌进行充分混合,置于聚苯乙烯板的上面,得到顶层;
(6)将底板、聚苯乙烯板和顶层放入压力机中进行压制成坯,压强保持在50-60Mpa;
(7)将成型坯在带有出气孔的烘干室内进行烘干,使烘干室内的温度保持在100℃,持续15小时,即得。

Claims (1)

1.具有防火和保温功能的吸音板的加工方法,其特征在于,吸音板包括以下重量份的各组份:
膨胀珍珠岩30-50份,水玻璃30-50份,玻璃纤维5-10份, 硼酸锌5-10份,  石灰粉  10-20份 ;
所述吸音板的加工方法包括以下步骤:
(1)选取的同一色度的膨胀珍珠岩用球磨机进行球磨,并使其颗粒的粒径为0.1-0.19mm,或者为1.1-3mm;
(2)将球磨完毕1/2重量份的膨胀珍珠岩与1/2重量份的石灰粉进行充分混合,并搅拌均匀;
(3)依次分别加入均为1/2重量份的水玻璃、玻璃纤维和硼酸锌;
(4)将上述混合料浆置入模具中并在压力机中进行轻压,使料浆不流动保持稳定即可,所需压力为20Mpa,得到底板;
(5) 在底板上放置一层聚苯乙烯板;
(6)将剩余的珍珠岩、水玻璃、玻璃纤维和硼酸锌进行充分混合,置于聚苯乙烯板的上面,得到顶层;
(6)将底板、聚苯乙烯板和顶层放入压力机中进行压制成坯,压强保持在50-60Mpa;
(7)将成型坯在带有出气孔的烘干室内进行烘干,使烘干室内的温度保持在50-100℃,持续15小时,即得。
CN 201110168445 2011-06-22 2011-06-22 具有防火和保温功能的吸音板及其加工方法 Expired - Fee Related CN102320805B (zh)