CN101994247A - 毛纱定型效果的测试方法 - Google Patents

毛纱定型效果的测试方法 Download PDF

Info

Publication number
CN101994247A
CN101994247A CN 201010279078 CN201010279078A CN101994247A CN 101994247 A CN101994247 A CN 101994247A CN 201010279078 CN201010279078 CN 201010279078 CN 201010279078 A CN201010279078 A CN 201010279078A CN 101994247 A CN101994247 A CN 101994247A
Authority
CN
China
Prior art keywords
yarn
reeled
hank
reeling frame
wool
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN 201010279078
Other languages
English (en)
Other versions
CN101994247B (zh
Inventor
陈丽芬
杨海军
曹秀明
何良
石小正
华玉龙
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Jiangsu Sunshine Co Ltd
Original Assignee
Jiangsu Sunshine Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Jiangsu Sunshine Co Ltd filed Critical Jiangsu Sunshine Co Ltd
Priority to CN2010102790783A priority Critical patent/CN101994247B/zh
Publication of CN101994247A publication Critical patent/CN101994247A/zh
Application granted granted Critical
Publication of CN101994247B publication Critical patent/CN101994247B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明涉及一种毛纱定型效果的测试方法,所述方法包括如下步骤:步骤一、取10只筒子作试样;步骤二、将试样筒子插在缕纱测长仪的纱锭插座上,退绕纱线至缕纱测长仪的摇纱框上,退绕满5圈后,将退绕好的纱线从试样筒子上剪断,摇纱框上的纱线就成绞纱状,称之为绞纱;步骤三、将摇纱框上的绞纱取出,保持绞纱垂直并处于自然无张力状态,静止5秒后松开绞纱下端,使绞纱自然加捻直到停止;步骤四、将手指放入绞纱下端绞纱开口处并拉紧绞纱,观察加捻方向后,松开手指,绞纱自动反向旋转退捻,记录退捻捻回数。采用本发明方法能测定毛纱的定型程度,通过测试,提前预知毛纱定型质量,并根据测试数据,制定合理的织造工艺参数,以提高纱线的织造效率,保证最终成品质量等。

Description

毛纱定型效果的测试方法
(一)技术领域
本发明涉及一种毛纱定型效果的测试方法。主要用于毛纱定型效果的测定。适用于评价羊毛的防缩性能。
(二)背景技术
近年来,随着毛纺产业链的不断拓展,产业分工不断细化,原来是中间过程产品,因产业分工的细化而成为最终贸易产品。对于毛纱厂而言,毛纱是最终成品,而对于织造厂或针织厂而言,毛纱就是重要的采购原材料。因此毛纱质量的高低直接影响着生产效率和最终产品的品质。
毛纱兼具成品或半成品的特性。目前,行业已制定有相关产品标准如《精梳机织毛纱》、《粗梳机织毛纱》、《精梳毛针织绒线》、《粗梳毛针织绒线》,标准中包括了毛纱支数、捻度、强力、条干等相关指标,在贸易和生产过程中,有时往往出现毛纱质量符合上述产品标准要求,但依然出现织造困难,织片弯斜等问题,究其原因,标准中没有纱线定型效果的相应指标,因纱线定型不足而造成的问题是比较严重的,纱线在织造过程中产生小辫子纱,严重影响坯布外观质量和带来最终成品疵点,造成结辫等,对针织加工而言除了织造效率的下降之外,还会带来下机织片因纱线定型不足而导致衣片向一个方向弯斜。因此毛纱的定型程度对于毛纱质量而言是非常重要的一项指标。由于目前产品标准中未包括纱线定型程度指标且目前没有相应测试方法,毛纱使用企业在生产时如不注意控制,往往到了最终成品才发现纱线定型问题,而且没有标准,供需双方难以就定型问题而有效交流。
(三)发明内容
本发明的目的在于克服上述不足,提供一种毛纱定型效果的测试方法。
本发明的目的是这样实现的:一种毛纱定型效果的测试方法,其特征在于所述方法包括如下步骤:
步骤一、取10只筒子作试样,每只测试2次;
步骤二、将试样筒子插在缕纱测长仪的纱锭插座上,退绕纱线至缕纱测长仪的摇纱框上,退绕圈数:5圈,退绕张力为(0.25±0.05)cN/tex,退绕满5圈后,将退绕好的纱线从试样筒子上剪断,摇纱框上的纱线就成绞纱状,称之为绞纱;
步骤三、一手捏住缕纱测长仪摇纱框上部夹纱部位处纱线,另一手捏住缕纱测长仪摇纱框下部夹纱部位处纱线,将摇纱框上的绞纱取出,保持绞纱垂直并处于自然无张力状态,静止5秒后松开绞纱下端,使绞纱自然加捻直到停止;
步骤四、将手指放入绞纱下端绞纱开口处并拉紧绞纱,观察加捻方向后,松开手指,绞纱由于存在回捻性,自动反向旋转退捻,并记录退捻捻回数;
步骤五、将缕长测长仪上绞纱逐绞取下按步骤三和步骤四规定测量;
试验结果计算
1)绞纱回捻数的计算
t = Σt s n
式中:
t——绞纱回捻数,捻,
∑ts——全部回捻数总和
n——试样数量;
试验结果分析
回捻数:0~5个,纱线定型效果好,织造效率高,织造无小辫子纱;
回捻数:6~10个,纱线定型效果一般,织造效率一般,织造需控制纱线张力,注意小辫子纱疵点;
回捻数:10个以上,纱线定型效果差,织造率率差,织造需调整纱线张力,严格防止小辫子纱。
测试原理:
纱线加捻后在松驰条件下,由于自身的退捻作用,一根对折(这是针对单根纱线而言,所谓对折,相当于把单根纱线折成圈,单根纱线的对折点就相当于绞纱的下端)的纱线沿对折点自然加捻,通过对其退捻测定捻回数。
本发明的有益效果是:
采用本发明方法能测定毛纱的定型程度,通过测试,提前预知毛纱定型质量,并根据测试数据,制定合理的织造工艺参数,以提高纱线的织造效率,保证最终成品质量等。
(四)附图说明
图1为本发明涉及的缕纱测长仪立体图。
图2为本发明涉及的毛纱定型效果图。
(五)具体实施方式
一、仪器与工具
1)缕纱测长仪
(1)结构原理:缕纱测长仪由摇纱框、纱锭插座、横动装置、张力秤和计数器等组成,如图1所示。纱线在标准规定的摇纱张力控制下均匀卷绕到摇纱框上,到预设的卷绕圈数自动停止。
(2)主要技术参数
1、试验纱管:6个
2、摇纱框周长:1000±1mm
3、摇纱框转速:30~300r.p.m
4、摇纱横动往复宽度:35mm
5、单根摇纱张力:0~100cN
6、外形尺寸(长×宽×高):YG086型:780×660×480mm
2)剪刀
在试验退绕纱线满5圈时,用于剪断纱线。
二、测试方法
本发明毛纱定型效果的测试方法,其包括如下步骤:
步骤一、取10只筒子作试样,每只测试2次。
步骤二、将试样筒子插在缕纱测长仪的纱锭插座上,退绕纱线至摇纱框上(摇纱框外形像古时的纺车,呈六边形立体状,退绕的纱线就是绕在此摇纱框上),圈数:5圈,张力为(0.25±0.05)cN/tex。满5圈后,用剪刀将绕好的纱线从试样筒子上剪断,摇纱框上的纱线就成绞纱状。纺织上习惯把周长一致的多根纱线组合称为“绞纱”。
步骤三、一手捏住缕纱测长仪摇纱框上部夹纱部位处纱线,另一手捏住缕纱测长仪摇纱框下部夹纱部位处纱线,将摇纱框上的绞纱轻轻取出,保持绞纱垂直并处于自然无张力状态,静止5秒后轻轻松开绞纱下端(指的是绞纱一端。绞线一般为条状,故存在两端的概念。试验时,取出绞纱时,是将绞纱沿长度方向大致垂直,所以有“下端”说法),使绞纱自然加捻直到停止。
步骤四、将手指放入绞纱下端绞纱开口处并拉紧绞纱(绞纱是一组封闭的纱线,所谓“下端绞纱开口处”,意指绞纱下端内部),观察加捻方向后,松开手指,绞纱由于存在回捻性,自动反向旋转退捻,并记录退捻捻回数。
步骤五、将缕长测长仪上绞纱逐绞取下按步骤三和步骤四规定测量
三、试验结果计算
1)绞纱回捻数的计算
t = Σt s n
式中:
t——绞纱回捻数,捻,
∑ts——全部回捻数总和
n——试样数量。
四、试验结果分析
回捻数:0~5个,纱线定型效果好,织造效率高,织造无小辫子纱;
回捻数:6~10个,纱线定型效果一般,织造效率一般,织造需控制纱线张力,注意小辫子纱疵点;
回捻数:10个以上,纱线定型效果差,织造率率差,织造需调整纱线张力,严格防止小辫子纱。
图2为本发明涉及的毛纱定型效果图,其中左边一幅图为定型效果好的毛纱样,中间一幅图为定型效果一般的毛纱样,右边一幅图为定型效果差的毛纱样。

Claims (1)

1.一种毛纱定型效果的测试方法,其特征在于所述方法包括如下步骤:
步骤一、取10只筒子作试样,每只测试2次;
步骤二、将试样筒子插在缕纱测长仪的纱锭插座上,退绕纱线至缕纱测长仪的摇纱框上,退绕圈数:5圈,退绕张力为0.25±0.05cN/tex,退绕满5圈后,将退绕好的纱线从试样筒子上剪断,摇纱框上的纱线就成绞纱状,称之为绞纱;
步骤三、一手捏住缕纱测长仪摇纱框上部夹纱部位处纱线,另一手捏住缕纱测长仪摇纱框下部夹纱部位处纱线,将摇纱框上的绞纱取出,保持绞纱垂直并处于自然无张力状态,静止5秒后松开绞纱下端,使绞纱自然加捻直到停止;
步骤四、将手指放入绞纱下端绞纱开口处并拉紧绞纱,观察加捻方向后,松开手指,绞纱由于存在回捻性,自动反向旋转退捻,并记录退捻捻回数;
步骤五、将缕长测长仪上绞纱逐绞取下按步骤三和步骤四规定测量;
试验结果计算
1)绞纱回捻数的计算
t = Σ t s n
式中:
t——绞纱回捻数,捻,
∑ts——全部回捻数总和
n——试样数量;
试验结果分析
回捻数:0~5个,纱线定型效果好,织造效率高,织造无小辫子纱;
回捻数:6~10个,纱线定型效果一般,织造效率一般,织造需控制纱线张力,注意小辫子纱疵点;
回捻数:10个以上,纱线定型效果差,织造率率差,织造需调整纱线张力,严格防止小辫子纱。
CN2010102790783A 2010-09-13 2010-09-13 毛纱定型效果的测试方法 Expired - Fee Related CN101994247B (zh)