CN101281306A - 液晶显示器硬式保护膜 - Google Patents

液晶显示器硬式保护膜 Download PDF

Info

Publication number
CN101281306A
CN101281306A CNA2008100968500A CN200810096850A CN101281306A CN 101281306 A CN101281306 A CN 101281306A CN A2008100968500 A CNA2008100968500 A CN A2008100968500A CN 200810096850 A CN200810096850 A CN 200810096850A CN 101281306 A CN101281306 A CN 101281306A
Authority
CN
China
Prior art keywords
film
liquid crystal
layer
reticulate pattern
lcd
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CNA2008100968500A
Other languages
English (en)
Other versions
CN101281306B (zh
Inventor
马慧军
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Suzhou Jin Fu technology Limited by Share Ltd
Original Assignee
SUZHOU JINFU NEW MATERIAL CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by SUZHOU JINFU NEW MATERIAL CO Ltd filed Critical SUZHOU JINFU NEW MATERIAL CO Ltd
Priority to CN2008100968500A priority Critical patent/CN101281306B/zh
Publication of CN101281306A publication Critical patent/CN101281306A/zh
Application granted granted Critical
Publication of CN101281306B publication Critical patent/CN101281306B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明涉及一种应用于保护液晶显示器的硬式保护膜,包括一层聚对苯二甲酸乙二醇酯层,其特征在于还具有一层聚乙烯网纹膜,所述液晶显示器硬式保护膜通过在聚对苯二甲酸乙二醇酯层的表面设置一层粘结剂层,然后与聚乙烯网纹膜的网纹面粘结复合而成。该硬式保护膜支撑力强且摩擦系数打,在使用本发明所述液晶显示器硬式保护膜保护液晶显示器时,将硬式保护膜的PE膜面面向液晶显示器并覆盖液晶模块的显示表面,使用胶带固定硬式保护膜的周边,可以防止液晶显示器被划伤,同时透气性强,耐高温高湿,抗静电。

Description

液晶显示器硬式保护膜
技术领域
本发明涉及一种复合膜,具体涉及一种应用于保护液晶显示器的硬式保护膜。
背景技术
液晶显示器通过如下方式进行生产:层压各种光学元件如玻璃衬底、液晶、偏振片(膜)、相位片(膜)、防反射膜以及类似元件,用由不锈钢金属板及其它类似金属制成的固定框架固定外围周边,此称为“企口”,从而构成液晶模块,液晶模块与其它组成部分一起安装并将所得结构体放入外壳中。为了防止装配和产品的发送过程中液晶模块被灰尘或其它脏物附着和污染,一般在液晶显示器的显示部分上覆盖一层表面保护膜(片)。在显示表面上覆盖一层表面保护粘性膜(层压膜),该粘性膜具有可脱开的并形成在该膜一面的整个区域上的粘性层,该粘性膜可以是聚乙烯膜、聚丙烯膜、氯化乙烯树脂膜、聚对苯二甲酸乙二醇酯膜和其它类似物,也可以将上述聚乙烯膜、聚丙烯膜、氯化乙烯树脂膜、聚对苯二甲酸乙二醇酯膜和其它类似物盖在液晶模块的显示表面,用胶带或其他方法固定粘性膜的外围周边。
保护膜以材质而论,可以简单地分为硬质及软质,硬质保护膜的典型代表有韩国产的SKC SH94,该产品的表面摩擦系数小,因此,在运输过程中,如果有小颗粒夹在保护膜和液晶显示器中间,在颠簸的情况下,小颗粒会与液晶显示器发生相对运动,从而划伤液晶显示器;软质的保护膜典型代表为日本三菱产的PC,这款产品比较柔软,但缺乏一定的支撑力。
而且,通常情况下的运输过程时间长,一般需要72~96小时,温度高,60℃左右,湿度高,70%左右,如果保护膜的设计不利于液晶显示器表面透气,则会导致水汽聚集在液晶显示器表面,从而影响显示器的显示效果。
发明内容
本发明目的是提供一种表面摩擦系数大,具有保护液晶显示器,防止液晶显示器在运输过程中被划伤,支撑力强,同时透气性良好,耐高温高湿的液晶显示器硬质保护膜。
为达到上述目的,本发明具体技术方案是,一种液晶显示器硬式保护膜,包括一层聚对苯二甲酸乙二醇酯层,其特征在于还具有一层聚乙烯网纹膜,所述液晶显示器硬式保护膜通过在聚对苯二甲酸乙二醇酯层的表面设置一层粘结剂层,然后与聚乙烯网纹膜的网纹面粘结复合而成。
上述技术方案中,聚对苯二甲酸乙二醇酯层(PET层)的作用在于提供一定的机械强度和支撑力,其厚度可以根据需求做相应的调整。
上述技术方案中,所述粘结剂可以选自公知的粘结剂,例如:丙烯类胶水,粘结剂层的厚度≤0.01cm。
聚乙烯网纹膜是通过在聚乙烯薄膜(PE薄膜)上设置粘胶剂层,然后使用滚花滚压粘胶剂层压出网纹,而且具有网纹结构的网纹面在纵深方向具有规整的凹陷空穴和凸起的结构;通常情况下,聚乙烯网纹膜被用于保护导光板、背光模组,通过将PE网纹膜的网纹面粘贴在导光板、背光模组的表面,从而保持导光板、背光模组的清洁;本技术方案并非将PE网纹膜粘贴在液晶显示器上,而是将PE网纹膜的网纹面与PET通过粘结剂粘结复合,其中构成PE网纹膜的粘胶剂层的厚度≥0.02CM,网纹空穴的深度≥0.02cm,粘结复合PET层与PE网纹膜的粘结剂层的厚度≤0.01cm,构成PE网格膜的PE膜厚度为0.03cm~0.05cm,复合过程中由于PET层以及PET层上的粘结剂层对PE网纹膜的凸起挤压,使得PE网纹膜的PE膜表面产生凸起,同样产生网纹结构。
优选的技术方案中,可以选用具有防静电功能的PE网纹膜,即在PE膜中加入抗静电剂。
在使用本发明所述液晶显示器硬式保护膜保护液晶显示器时,将硬式保护膜的PE膜面面向液晶显示器并覆盖液晶模块的显示表面,使用胶带固定硬式保护膜的周边。
由于上述技术方案运用,本发明与现有技术相比具有下列优点:
1.因为PE膜本身柔软,其表面硬度为0.4~0.6,而且本发明中PE膜表面具有凸起和网纹结构,其表面摩擦系数约为0.5,所以,当小颗粒夹在硬式保护膜和液晶模块的显示表面时,小颗粒与保护膜表面和液晶模块的显示表面在颠簸的情况下也不易发生相对运动,同时,受到外力的挤压作用时,小颗粒会陷入柔软的PE膜内,因此,在运输过程中,可以防止液晶模块的显示表面被划伤;
2.因为PE膜的表面具有凸起和网纹结构,在运输过程中,高温高湿情况下,这样的结构有利于透气,所以可以防止水汽在液晶模块的显示表面聚集,防止水汽影响最终液晶显示器的显示效果;
3.本发明可以通过调节PET的厚度来调整产品的支撑力,同时由于PE膜柔软,因此,支撑力强且表面柔软,同时本发明耐高温高湿。
附图说明
图1是实施例中复合前的PET膜及粘结剂层的剖面示意图;
图2是实施例中复合前的PE网纹膜的剖面示意图;
图3是实施例中复合前的PE网纹膜的PE面示意图;
图4是实施例中复合前的PE网纹膜的凸起和空穴示意图;
图5是实施例中复合后硬式保护膜的剖面示意图。
其中,1、PET层;2、粘结剂层;3、PE网纹膜的PE层;4、PE网纹膜的粘胶剂层;5、PE网纹膜的空穴;6、PE网纹膜的凸起;7、凸起结构。
具体实施方式
下面结合附图及实施例对本发明作进一步描述:
实施例一
1、如图1所示,选用0.125cm厚的PET薄膜,构建PET层1,在PET薄膜上涂布一层厚度为0.01cm的胶水,形成粘结剂层2;
2、如图2、3和4所示,选择具有抗静电功能的PE网纹膜,PE网纹膜的PE层3厚度为0.03cm,PE网纹膜的粘胶剂层4厚度为0.02cm,PE网纹膜的凸起6的顶端和空穴的底端之间的垂直距离为0.02cm;
3、使用压滚机复合涂布有胶水层的PET薄膜和PE网纹膜,复合的压力为7kg/m2,构成液晶显示器的硬式保护膜,经过滚压复合后,所述硬式保护膜的PE层表面具有凸起结构7,如图5所示;
4、将硬式保护膜的PE膜面面向液晶显示器并覆盖液晶模块的显示表面,使用胶带固定硬式保护膜的周边,用于保护液晶显示器,防止液晶模块的显示表面被划伤,被污染以及被水气影响,还具有防静电功能。
实施例二
1、如图1所示,选用0.075cm厚的PET薄膜;
2、如图2、3和4所示,选择PE网纹膜,其PE层厚度为0.04cm,粘胶剂层厚度为0.025cm,空穴的深度为0.025cm;
3、使用涂布机在PET薄膜上涂布一层厚度为0.008cm的胶水,然后利用复合滚将涂布有胶水的PET薄膜和PE网纹膜复合,复合压力为6kg/m2,构成液晶显示器的硬式保护膜,经过滚压复合后,所述硬式保护膜的PE层表面具有凸起结构,如图5所示;
4、将硬式保护膜的PE膜面面向液晶显示器并覆盖液晶模块的显示表面,使用胶带固定硬式保护膜的周边,用于保护液晶显示器,防止液晶模块的显示表面被划伤,被污染以及被水气影响。

Claims (6)

1.一种液晶显示器硬式保护膜,包括一层聚对苯二甲酸乙二醇酯层,其特征在于:还具有一层聚乙烯网纹膜,聚乙烯网纹膜的网纹面经一层粘结剂层与聚对苯二甲酸乙二醇酯层复合。
2.根据权利要求1所述的液晶显示器硬式保护膜,其特征在于:聚乙烯网纹膜的空穴深度≥0.02cm,聚乙烯膜的厚度为0.03cm~0.05cm。
3.根据权利要求1所述的液晶显示器硬式保护膜,其特征在于:设置在聚对苯二甲酸乙二醇酯层的表面的粘结剂层的厚度≤0.01cm。
4.根据权利要求2和3所述的液晶显示器硬式保护膜,其特征在于:聚乙烯网纹膜的空穴深度为0.02cm,聚乙烯膜的厚度为0.03cm,设置在聚对苯二甲酸乙二醇酯层的表面的粘结剂层的厚度为0.01cm。
5.根据权利要求1所述的液晶显示器硬式保护膜,其特征在于:聚对苯二甲酸乙二醇酯层与聚乙烯网纹膜通过粘结剂层复合后聚乙烯网纹膜的聚乙烯膜的表面具有凸起和网纹结构。
6.根据权利要求1所述的液晶显示器硬式保护膜,其特征在于:所述聚乙烯网纹膜中含有防静电剂。
CN2008100968500A 2008-05-06 2008-05-06 液晶显示器硬式保护膜 Active CN101281306B (zh)