CN101214637B - 玻璃磨边轮 - Google Patents

玻璃磨边轮 Download PDF

Info

Publication number
CN101214637B
CN101214637B CN2008100490908A CN200810049090A CN101214637B CN 101214637 B CN101214637 B CN 101214637B CN 2008100490908 A CN2008100490908 A CN 2008100490908A CN 200810049090 A CN200810049090 A CN 200810049090A CN 101214637 B CN101214637 B CN 101214637B
Authority
CN
China
Prior art keywords
resin
parts
orders
coupling agent
polyvinyl butyral
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN2008100490908A
Other languages
English (en)
Other versions
CN101214637A (zh
Inventor
李士欣
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
New Anhua (Zhengzhou) Abrasives Co., Ltd.
Original Assignee
Anhua Zhengzhou Abrasives Co ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Anhua Zhengzhou Abrasives Co ltd filed Critical Anhua Zhengzhou Abrasives Co ltd
Priority to CN2008100490908A priority Critical patent/CN101214637B/zh
Publication of CN101214637A publication Critical patent/CN101214637A/zh
Application granted granted Critical
Publication of CN101214637B publication Critical patent/CN101214637B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种玻璃磨边轮,由下述重量份配比的原料制备而成:a、配比:白刚玉粉料:170份,500目以上;偶联剂:0.5-1份;EP树脂:21-29份;PF树脂:20-32份,320目以上;硅酸盐填料:40-60份,320目以上;聚乙烯醇缩丁醛:0.5-2份;b、制备方法:1,首先将白刚玉粉料做混前偶联剂处理,然后加入EP树脂混合均匀,再加入PF树脂、填料、聚乙烯醇缩丁醛进行充分搅拌;2,将第一步所得混合料装入模具内进行冷压成型,压力13MPa以上;3,将第二步制成的毛坯放入烘箱里加热,然后停止加热,自然冷却即得成品。本发明优点在于通过科学的原料配比选择,因此在对玻璃边进行几何图形修整的同时还起到了抛光抛亮的效果,使用方便快捷。

Description

玻璃磨边轮
技术领域
本发明涉及磨料磨具,尤其是涉及玻璃磨边轮。
背景技术
目前对玻璃毛边的修整多采用普通砂轮来完成,由于玻璃所具有的特性,普通砂轮对玻璃毛边的修整常常出现掉块而影响玻璃边沿的平整度,并且不具有抛光功能,需要抛光还必须采用专用抛光轮来完成。
发明内容
本发明目的在于提供一种具有修整、抛光功能的玻璃磨边轮。
为实现上述目的,本发明可采取下述技术方案:
本发明所述的玻璃磨边轮,它由下述重量份配比的原料制备而成:
a、原料配比:
白刚玉粉料:170份,500目以上;偶联剂:0.5-1份;EP树脂:21-29份;
PF树脂:20-32份,320目以上;硅酸盐填料:40-60份,320目以上;
聚乙烯醇缩丁醛:0.5-2份;
b、制备方法:
第一步,首先将白刚玉粉料做混前偶联剂处理,然后加入EP树脂混合均匀,再加入PF树脂、填料、聚乙烯醇缩丁醛进行充分搅拌;
第二步,将第一步所得混合料装入模具内进行冷压成型,压力13MPa以上;
第三步,将第二步制成的毛坯放入烘箱里加热,加热过程为:
80℃,2h→100℃,2h→120℃,1h→140℃,1h→150℃,1h→160℃,1h→180℃,3h;然后停止加热,自然冷却即得成品。
本发明优点在于通过科学的原料配比选择,因此在对玻璃边进行几何图形修整的同时还起到了抛光抛亮的效果,使用方便快捷,并杜绝了对玻璃毛边修整过程中出现的掉块现象发生,使修整后玻璃边的平整度、光洁度得以大幅度提高。
具体实施方式
实施例1:
本发明所述的玻璃磨边轮,由下述重量份配比的原料制备而成:
a、原料配比:
白刚玉粉料:170份,500目以上;偶联剂:0.5份;EP树脂:21份;
PF树脂:20份,320目以上;硅酸盐填料:40份,320目以上;
聚乙烯醇缩丁醛:0.5份。
b、制备方法:
第一步,首先将白刚玉粉料做混前偶联剂处理,然后加入EP树脂混合均匀,再加入PF树脂、填料、聚乙烯醇缩丁醛进行充分搅拌;
第二步,将第一步所得混合料装入模具内进行冷压成型,压力13MPa以上;
第三步,将第二步制成的毛坯放入烘箱里加热,加热过程为:
80℃,2h→100℃,2h→120℃,1h→140℃,1h→150℃,1h→160℃,1h→180℃,3h;然后停止加热,自然冷却即得成品。
实施例2:
本发明所述的玻璃磨边轮,由下述重量份配比的原料制备而成:
a、原料配比:
白刚玉粉料:170份,500目以上;偶联剂:0.8份;EP树脂:26份;
PF树脂:26份,320目以上;硅酸盐填料:50份,320目以上;
聚乙烯醇缩丁醛:1份。
b、制备方法:
第一步,首先将白刚玉粉料做混前偶联剂处理,然后加入EP树脂混合均匀,再加入PF树脂、填料、聚乙烯醇缩丁醛进行充分搅拌;
第二步,将第一步所得混合料装入模具内进行冷压成型,压力13MPa以上;
第三步,将第二步制成的毛坯放入烘箱里加热,加热过程为:
80℃,2h→100℃,2h→120℃,1h→140℃,1h→150℃,1h→160℃,1h→180℃,3h;然后停止加热,自然冷却即得成品。
实施例3:
本发明所述的玻璃磨边轮,由下述重量份配比的原料制备而成:
a、原料配比:
白刚玉粉料:170份,500目以上;偶联剂:1份;EP树脂:29份;
PF树脂:32份,320目以上;硅酸盐填料:60份,320目以上;
聚乙烯醇缩丁醛2份。
b、制备方法:
第一步,首先将白刚玉粉料做混前偶联剂处理,然后加入EP树脂混合均匀,再加入PF树脂、填料、聚乙烯醇缩丁醛进行充分搅拌;
第二步,将第一步所得混合料装入模具内进行冷压成型,压力13MPa以上;
第三步,将第二步制成的毛坯放入烘箱里加热,加热过程为:
80℃,2h→100℃,2h→120℃,1h→140℃,1h→150℃,1h→160℃,1h→180℃,3h;然后停止加热,自然冷却即得成品。

Claims (4)

1.一种玻璃磨边轮,其特征在于:它由下述重量份配比的原料制备而成:
a、原料配比:
白刚玉粉料:170份,500目以上;偶联剂:0.5-1份;EP树脂:21-29份;
PF树脂:20-32份,320目以上;硅酸盐填料:40-60份,320目以上;
聚乙烯醇缩丁醛:0.5-2份;
b、制备方法:
第一步,首先将白刚玉粉料做混前偶联剂处理,然后加入EP树脂混合均匀,再加入PF树脂、填料、聚乙烯醇缩丁醛进行充分搅拌;
第二步,将第一步所得混合料装入模具内进行冷压成型,压力13MPa以上;
第三步,将第二步制成的毛坯放入烘箱里加热,加热过程为:
80℃,2h→100℃,2h→120℃,1h→140℃,1h→150℃,1h→160℃,1h→180℃,3h;然后停止加热,自然冷却即得成品。
2.根据权利要求1所述的玻璃磨边轮,其特征在于:所述原料配比为:
白刚玉粉料:170份,500目以上;偶联剂:0.5份;EP树脂:21份;
PF树脂:20份,320目以上;硅酸盐填料:40份,320目以上;
聚乙烯醇缩丁醛:0.5份。
3.根据权利要求1所述的玻璃磨边轮,其特征在于:所述原料配比为:
白刚玉粉料:170份,500目以上;偶联剂:0.8份;EP树脂:26份;
PF树脂:26份,320目以上;硅酸盐填料:50份,320目以上;
聚乙烯醇缩丁醛:1份。
4.根据权利要求1所述的玻璃磨边轮,其特征在于:所述原料配比为:
白刚玉粉料:170份,500目以上;偶联剂:1份;EP树脂:29份;
PF树脂:32份,320目以上;硅酸盐填料:60份,320目以上;
聚乙烯醇缩丁醛2份。
CN2008100490908A 2008-01-16 2008-01-16 玻璃磨边轮 Expired - Fee Related CN101214637B (zh)