CN100480346C - Anti-rust coating agent and method for preparing the same - Google Patents

Anti-rust coating agent and method for preparing the same Download PDF

Info

Publication number
CN100480346C
CN100480346C CNB2004100924631A CN200410092463A CN100480346C CN 100480346 C CN100480346 C CN 100480346C CN B2004100924631 A CNB2004100924631 A CN B2004100924631A CN 200410092463 A CN200410092463 A CN 200410092463A CN 100480346 C CN100480346 C CN 100480346C
Authority
CN
China
Prior art keywords
kilograms
coating agent
ethanol
rust
acetone
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CNB2004100924631A
Other languages
Chinese (zh)
Other versions
CN1664033A (en
Inventor
徐大财
王澍
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Xu Dacai
Original Assignee
JIANGSU CHAMPION COATING MATERIAL INDUSTRY Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by JIANGSU CHAMPION COATING MATERIAL INDUSTRY Ltd filed Critical JIANGSU CHAMPION COATING MATERIAL INDUSTRY Ltd
Priority to CNB2004100924631A priority Critical patent/CN100480346C/en
Publication of CN1664033A publication Critical patent/CN1664033A/en
Application granted granted Critical
Publication of CN100480346C publication Critical patent/CN100480346C/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The present invention provides an anti-rust coating agent which chooses polyhydroxy high polymer as principal film-forming agent and can be formed to high stable status and not breadcrust film matched with a plurality of film build auxiliaries. The anti-rust coating agent includes the following materials with weight percent: colophony glyceride 0.3-5%, formaldehyde-phenol resin 3-12%, epoxy resins 2-10%, polyvinyl butyral 1-6%, acetone 3-8%, ethanol 38-53%, n-butyl alcohol 1-7%, phosphoric acid 1-5%, and the residual is additive agent. The coating agent of the invention can effectively chemical and physical combine with metal bases such as steel, iron and aluminum, thereby can conquer the paints doff problem for conventional paints, enhance the anti-rust property, and improve use life, and is a novel anti-rust coating agent product.

Description

Anti-rust coating agent and preparation method thereof
Technical field
The present invention relates to a kind of anti-rust coating agent, be widely used in the antirust waterproofing protections of product such as steel, iron, aluminium, zinc, boats and ships, lathe, electromechanics, electronics, vehicle, woodenware, building.
Background technology
Paint is being also referred to as coating, and the kind of paint is numerous, and its performance also has nothing in common with each other.The coating quantity that wherein is used for the antirust covering with paint aspect on the metal productss such as iron and steel, aluminium, zinc is more, but does not find as yet that both at home and abroad a kind of paint overall target (as sticking power, shock resistance, snappiness etc.) possesses the product of optimum performance simultaneously.Whether these important indicators are really up to the mark, are the principal elements that influences pull-away.At present, cause the metal products corrosion and scrap, become a very big difficult problem because the paint film crackle peels off.
The increasing cost is not stinted in order to prevent depainting by present enterprises such as vehicle, machinery, household electrical appliances, and the various treatment process before before japanning the metal products matrix being carried out application have expended a large amount of funds, make painting cost be higher than metal body far away.However, often still be difficult to avoid be given a shock, clash into the phenomenon that depainting occurs because of product.
Among numerous paint, cause except the ubiquity depainting the corrosion of metal, also exist because of obnoxious flavoures such as poisonous metal elements such as leaded, chromium, mercury and benzene, make coating process become harmful work post, human body and environment are caused severe contamination.Owing to traditional paint easy skinning in the shelf lives causes downgrade to cause scrapping, only this item can be wasted the product more than 30% again, and it is inestimable especially to apply the loss that causes in the process.Therefore solve the difficult problem of paint existence at present, research and develop a kind of novel paint and be imminent.
Summary of the invention
The present invention be directed to the difficult problem that the protection of anti-corrosion of metal such as present iron and steel body exists, and development synthetic a kind of with the poly-hydroxy high molecular polymer as main membrane-forming agent, and with compound high surely state, the film forming anti-rust coating agent of skinning not of being made into of multiple film coalescence aid.The preparation method that this anti-rust coating agent also is provided of the present invention.
The objective of the invention is to realize by following measure:
A kind of anti-rust coating agent comprises following raw materials by weight percent:
Rosin glyceride 0.3-5%, resol 3-12%, Resins, epoxy 2-10%, polyvinyl butyral acetal 1-6%, acetone 3-8%, ethanol 38-53%, propyl carbinol 1-7%, phosphatase 11-5%, surplus is an additive.
Wherein, described additive is MALEIC ANHYDRIDE, phenylformic acid, dibutyl phthalate (DBP), Viscotrol C.
The preparation method of anti-rust coating agent of the present invention, its making processes is as follows:
Get above-mentioned raw materials by weight percent, earlier with resol, Resins, epoxy under 180-220 ℃ condition polyreaction 0.2-3 hour, the mixture of the rosin glyceride that adds, part ethanol, polyvinyl butyral acetal, the ethanol of adding residue again, propyl carbinol, acetone, phosphoric acid, additive are mixed into transparent monomers finished product coating; Pigment is added in the monomer finished product coating, high speed dispersion, grinding, filtration pump in the toning still and are mixed into versicolor coating again.
Metallic matrixes such as realization of the present invention and steel, iron, aluminium are Chemical bond and physical bond effectively, thereby overcomes the depainting problem of traditional paint, strengthens rustless property, improves the novel antirust liniment product in work-ing life.This product is made solvent with food grade alcohol and non-toxic alcohol, and the process that applies is non-volatile to go out obnoxious flavoures such as benzene, toluene, and poisonous metal element such as not leaded in the product, chromium, mercury forms environment-friendly type coating.Utilization rust transformation technology makes product save phosphatization and the processing of sun levelization before paint coating lathe turner simultaneously, becomes harmful work post and is harmless work post.
In order to overcome the shortcoming of the easy skinning downgrade of traditional paint, anti-rust coating agent of the present invention adopts alcohol-based solvent to add advanced complex process technology, it is doubly above and skinning not reaches and saves the purpose that paint reduces painting cost that the shelf lives that makes product prolongs 3-5 than traditional paint.
Anti-rust coating agent of the present invention is with the high adhesive force transparent monomers and have the good supporting of acidproof, alkaline-resisting, high temperature resistant, antirust, waterproof, insulation multifrequency nature and other paint, can be widely used in steel, iron, aluminium, zinc, boats and ships, lathe, electromechanics, electronics, the antirust waterproofing protection of vehicle product.The on-mechanical behavior of filming does not have the phenomenon that glue falls under the general environment condition.
Anti-rust coating agent of the present invention with quality high stable, self-drying type, good leveling property, apply conveniently, as new series coating such as rust-inhibiting paint, rust-proofing primer, preliminary larquerings, will become the renewal product of metal finishing.
The synopsis of anti-rust coating agent of the present invention and existing product performance:
Content Form Sticking power Coating method Contain harmful composition The quality quality guaranteed period
Existing product The two components of colorant 1 grade Need phosphatization, the processing of sun levelization before the coating construction Obnoxious flavoures such as harmful elements such as leaded, chromium, mercury and benzene 6 months
Anti-rust coating agent Transparent single-component colorant single-component <1 grade Do not need phosphatization, the processing of sun levelization before containing rust transformation function coating construction Do not contain harmful metallic element and obnoxious flavour More than 2 years
Embodiment
The invention will be further described below in conjunction with accompanying drawing:
Embodiment 1
The preparation method of anti-rust coating agent of the present invention, its making processes is as follows:
Get 2.6 kilograms of rosin glycerides, 10 kilograms in resol, 8 kilograms of Resins, epoxy, 4 kilograms of polyvinyl butyral acetals, 8 kilograms in acetone, 53 kilograms of ethanol, 3 kilograms of propyl carbinols, 2 kilograms of phosphoric acid, 9.4 kilograms of MALEIC ANHYDRIDE.
Earlier with resol, Resins, epoxy polyreaction 0.2 hour under 180 ℃ condition, the mixture that adds rosin glyceride, part ethanol (its effect is that rosin glyceride and polyvinyl butyral acetal are reconciled into one), polyvinyl butyral acetal, the ethanol of adding residue again, propyl carbinol, acetone, phosphoric acid, MALEIC ANHYDRIDE are mixed into transparent monomers finished product coating; Pigment is added in the monomer finished product coating, high speed dispersion, grinding, filtration pump in the toning still and are mixed into versicolor coating again.
Embodiment 2
Other condition is constant, wherein get 0.3 kilogram of rosin glyceride, 3 kilograms in resol, 2 kilograms of Resins, epoxy, 1 kilogram of polyvinyl butyral acetal, 8 kilograms in acetone, 53 kilograms of ethanol, 7 kilograms of propyl carbinols, 5 kilograms of phosphoric acid, 20.7 kilograms of MALEIC ANHYDRIDE, other presses embodiment 1, adds red pigment and makes red coating.
Embodiment 3
The preparation method of anti-rust coating agent of the present invention: get 3 kilograms of rosin glycerides, 9 kilograms in resol, 10 kilograms of Resins, epoxy, 5 kilograms of polyvinyl butyral acetals, 5 kilograms in acetone, 44 kilograms of ethanol, 3 kilograms of propyl carbinols, phosphatase 24 kilogram, 17 kilograms of MALEIC ANHYDRIDE.
Earlier with resol, Resins, epoxy polyreaction 1 hour under 200 ℃ condition, the rosin glyceride, part ethanol, the polyvinyl butyral acetal mixture that add, the ethanol of adding residue again, propyl carbinol, acetone, phosphoric acid, MALEIC ANHYDRIDE are mixed into transparent monomers finished product coating; Pigment is added in the monomer finished product coating, high speed dispersion, grinding, filtration pump in the toning still and are mixed into versicolor coating again.
Embodiment 4
Other condition is constant, wherein get 5 kilograms of rosin glycerides, 12 kilograms in resol, 10 kilograms of Resins, epoxy, 6 kilograms of polyvinyl butyral acetals, 3 kilograms in acetone, 38 kilograms of ethanol, 1 kilogram of propyl carbinol, 7 kilograms of phosphoric acid, 18 kilograms in phenylformic acid, other presses embodiment 3, adds yellow ultramarine and makes xanchromatic coating.
Embodiment 5
Get 2.5 kilograms of rosin glycerides, 11 kilograms in resol, 9 kilograms of Resins, epoxy, 5.5 kilograms of polyvinyl butyral acetals, 6.5 kilograms in acetone, 53 kilograms of ethanol, 3.5 kilograms of propyl carbinols, 3 kilograms of phosphoric acid, 6 kilograms of dibutyl phthalate (DBP)s.
Earlier with resol, Resins, epoxy polyreaction 3 hours under 220 ℃ condition, the rosin glyceride, part ethanol, the polyvinyl butyral acetal mixture that add, the ethanol of adding residue again, propyl carbinol, acetone, phosphoric acid, dibutyl phthalate (DBP) are mixed into transparent monomers finished product coating; Pigment is added in the monomer finished product coating, high speed dispersion, grinding, filtration pump in the toning still and are mixed into versicolor coating again.
Embodiment 6
Other condition is constant, wherein get 2 kilograms of rosin glycerides, 8 kilograms in resol, 7 kilograms of Resins, epoxy, 3.5 kilograms of polyvinyl butyral acetals, 5.5 kilograms in acetone, 40 kilograms of ethanol, 4 kilograms of propyl carbinols, 5 kilograms of phosphoric acid, Viscotrol C 25, other presses embodiment 5, adds veridian and makes green coating.
Embodiment 7
Other condition is constant, wherein get 5 kilograms of rosin glycerides, 12 kilograms in resol, 10 kilograms of Resins, epoxy, 6 kilograms of polyvinyl butyral acetals, 8 kilograms in acetone, 44 kilograms of ethanol, 7 kilograms of propyl carbinols, 5 kilograms of phosphoric acid, 3 kilograms of Viscotrol C, other presses embodiment 5, adds veridian and makes green coating.
Embodiment 8
Other condition is constant, wherein get 4 kilograms of rosin glycerides, 11 kilograms in resol, 9 kilograms of Resins, epoxy, 5 kilograms of polyvinyl butyral acetals, 7 kilograms in acetone, 51 kilograms of ethanol, 6 kilograms of propyl carbinols, the phosphatase 24 kilogram, 3 kilograms in phenylformic acid, other presses embodiment 5, adds pink pigment and makes green coating.
Embodiment 9
Other condition is constant, wherein get 5 kilograms of rosin glycerides, 11 kilograms in resol, 10 kilograms of Resins, epoxy, 6 kilograms of polyvinyl butyral acetals, 8 kilograms in acetone, 40 kilograms of ethanol, 7 kilograms of propyl carbinols, 5 kilograms of phosphoric acid, 8 kilograms of MALEIC ANHYDRIDE, other presses embodiment 5, adds veridian and makes green coating.
Embodiment 10
Get 0.3 kilogram of rosin glyceride, 3 kilograms in resol, 2 kilograms of Resins, epoxy, 1 kilogram of polyvinyl butyral acetal, 3 kilograms in acetone, 38 kilograms of ethanol, 1 kilogram of propyl carbinol, phosphatase 11 kilogram, 50.7 kilograms of dibutyl phthalate (DBP)s.Other presses embodiment 5, adds veridian and makes green coating.

Claims (2)

1, a kind of anti-rust coating agent comprises following raw materials by weight percent:
Rosin glyceride 0.3-5%, resol 3-12%, Resins, epoxy 2-10%, polyvinyl butyral acetal 1-6%, acetone 3-8%, ethanol 38-53%, propyl carbinol 1-7%, phosphatase 11-5%, surplus is an additive; Wherein, described additive is MALEIC ANHYDRIDE, phenylformic acid, dibutyl phthalate (DBP) or Viscotrol C.
2, the preparation method of the described anti-rust coating agent of claim 1, its making processes is as follows:
Get above-mentioned raw materials by weight percent, earlier with resol, Resins, epoxy under 180-220 ℃ condition polyreaction 0.2-3 hour, the mixture that adds rosin glyceride, part ethanol, polyvinyl butyral acetal, the ethanol of adding residue again, propyl carbinol, acetone, phosphoric acid, additive are mixed into transparent monomers finished product coating.
CNB2004100924631A 2004-12-14 2004-12-24 Anti-rust coating agent and method for preparing the same Expired - Fee Related CN100480346C (en)