CN100437362C - 彩色复印机用青色碳粉及其制备方法 - Google Patents

彩色复印机用青色碳粉及其制备方法 Download PDF

Info

Publication number
CN100437362C
CN100437362C CNB2006100411235A CN200610041123A CN100437362C CN 100437362 C CN100437362 C CN 100437362C CN B2006100411235 A CNB2006100411235 A CN B2006100411235A CN 200610041123 A CN200610041123 A CN 200610041123A CN 100437362 C CN100437362 C CN 100437362C
Authority
CN
China
Prior art keywords
parts
compound
vibrin
carbon powder
ching
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CNB2006100411235A
Other languages
English (en)
Other versions
CN1912753A (zh
Inventor
周学良
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Wuxi Jiateng Magnetic Powder Co., Ltd.
Original Assignee
周学良
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 周学良 filed Critical 周学良
Priority to CNB2006100411235A priority Critical patent/CN100437362C/zh
Publication of CN1912753A publication Critical patent/CN1912753A/zh
Application granted granted Critical
Publication of CN100437362C publication Critical patent/CN100437362C/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开一种彩色复印机用青色碳粉及其制备方法。它是用80~90份的聚酯树脂、5~10份的聚丙烯蜡、3~9份的电荷调节剂、7~10份的酞青蓝、2~4份的二甲基二氯硅烷和7~10份的六甲基二硅氮烷,经混炼、挤塑、粉碎和过筛等步骤而制成。用这种青色碳粉与黄、红、黑三种彩色复印机用碳粉组成4种基本颜色,能形成千上万种颜色,不仅复印的文稿和图像清晰、不褪色,还可降低使用成本、减少复印机的故障率。

Description

彩色复印机用青色碳粉及其制备方法
技术领域
本发明涉及一种碳粉及其制备方法。具体说,是用来复印彩色文稿或彩色图片的彩色复印机用青色碳粉及其制备方法。
背景技术
目前,彩色复印机上使用的碳粉,其主要成份树脂都是采用苯乙烯和丙烯酸二元共聚物。利用这种树脂作为主要原料制成的彩色复印机用碳粉,存在以下问题:生产过程中,难以粉碎,颗粒较大且形状不规则。由于颗粒较大且形状不规则,复印时,难以均匀地复着在纸上,不仅成像效果较差,而且碳粉的消耗量多、使用成本较高。又由于苯乙烯和丙烯酸二元共聚物有异味,使得制成的碳粉亦有异味,不利于环境保护。
发明内容
本发明要解决的问题是提供一种彩色复印机用青色碳粉。这种青色碳粉,不仅颗粒小、形状规则、成像效果好,而且复印时消耗量少、使用成本低。
本发明要解决的另一个问题是提供一种制备彩色复印机用红色碳粉的方法。
为解决上述问题,本发明采取以下技术解决方案:
本发明的彩色复印机用红色碳粉由以下重量份数的原料组成:
聚酯树脂80~90份;聚丙烯蜡5~10份;电荷调节剂3~9份;酞青蓝7~10份;二甲基二氯硅烷2~4份;六甲基二硅氮烷7~10份。
其中的聚酯树脂是按照对苯二甲酸酯∶间苯二甲酸酯=2∶8的比例反应而成的二元共聚物;电荷调节剂是金属水杨酸铬合物或金属偶氮铬合物。
制备彩色复印机用青色碳粉的方法包括以下步骤:
(1)先将聚酯树脂、聚丙烯蜡、酞青蓝和电荷调节剂倒入混炼机中,经均匀混合,制成混合料;
(2)再将上述混合料投入挤塑机中,在90~150℃的温度下将混合料挤出压制成片;然后,将片状混合料冷却至40~45℃并粉碎成碎片;
(3)之后,用粉碎机将上述碎片粉碎成粒径为30~50μm的碎粉;
(4)之后,用粉碎机对上述碎粉进行进一步粉碎,并依次进行分级、分离、收集,得到粒径为7~9μm的半成品颗粒;
(5)再之后,加入二甲基二氯硅烷和六甲基二硅氮烷,用850~950转/分钟的混炼机混合3~4分钟,使其流动性大于20%;
(6)最后,用200~250目筛网过筛,制成彩色复印机用青色碳粉。
采用以上方案,具有以下优点:
由于本发明的青色碳粉所用树脂为聚酯树脂,该树脂是按照对苯二甲酸酯∶间苯二甲酸酯=2∶8的比例反应而成,用这种树脂与聚丙烯蜡、电荷调节剂、酞青蓝、二甲基二氯硅烷和六甲基二硅氮烷等原料一起,经混炼、挤塑、粉碎和过筛等步骤制成的青色碳粉,生产过程中容易粉碎,颗粒较小且比较规则。由于颗粒较小且比较规则,复印时,与黄、红、黑色碳粉组成四种基本色,能均匀地附着在纸上,不仅成像效果好,而且消耗量少、使用成本较低。又由于所用树脂为聚酯树脂,且该树脂是按照对苯二甲酸酯∶间苯二甲酸酯=2∶8的比例反应而成,其中的对苯二甲酸酯和间苯二甲酸酯无异味,使得制成的青色碳粉也无异味,有利于环境保护。
具体实施方式
第一个实施例
选取80份的聚酯树脂、5份的聚丙烯蜡、3份的电荷调节剂、7份的酞青蓝、2份的二甲基二氯硅烷和7份的六甲基二硅氮烷,待用。
先将聚酯树脂、聚丙烯蜡、电荷调节剂和酞青蓝倒入混炼机中,经均匀混合,制成混合料;
再将上述混合料投入挤塑机中,在95℃的温度下将混合料剂出,压制成片;然后,将片状混合料冷却至40℃,并粉碎成碎片;
之后,用粉碎机将上述碎片粉碎成粒径为30μm的碎粉;
之后,用压力为5.5kg/m3压缩空气在流化床粉碎机中对上述碎粉进行气流粉碎并用5500转/分钟的分级机进行分级、用旋风分离器进行分离、用捕集器进行收集,得到粒径为7~9μm的半成品颗粒;
再之后,加入二甲基二氯硅烷和六甲基二硅氮烷,用850转/分钟的混炼机混合3分钟,使其流动性大于20%;
最后,用200目筛网过筛,制成彩色复印机用青色碳粉。
其中:聚酯树脂是按照对苯二甲酸酯∶间苯二甲酸酯=2∶8的比例反应而成的二元共聚物;电荷调节剂是金属水杨酸铬合物。
第二个实施例
选取85份的聚酯树脂、8份的聚丙烯蜡、6份的电荷调节剂、9份的酞青蓝、3份的二甲基二氯硅烷和8份的六甲基二硅氮烷,待用。
先将聚酯树脂、聚丙烯蜡、电荷调节剂和酞青蓝倒入混炼机中,经均匀混合,制成混合料;
再将上述混合料投入挤塑机中,在120℃的温度下将混合料剂出,压制成片;然后,将片状混合料冷却至43℃,并粉碎成碎片;
之后,用粉碎机将上述碎片粉碎成粒径为40μm的碎粉;
之后,用压力为6.8kg/m3压缩空气在流化床粉碎机中对上述碎粉进行气流粉碎并用5800转/分钟的分级机进行分级、用旋风分离器进行分离、用捕集器进行收集,得到粒径为7~9μm的半成品颗粒;
再之后,加入二甲基二氯硅烷和六甲基二硅氮烷,用900转/分钟的混炼机混合3分钟,使其流动性大于20%;
最后,用230目筛网过筛,制成彩色复印机用青色碳粉。
其中:聚酯树脂是按照对苯二甲酸酯∶间苯二甲酸酯=2∶8的比例反应而成的二元共聚物;电荷调节剂是金属偶氮铬合物。
第三个实施例
选取90份的聚酯树脂、10份的聚丙烯蜡、9份的电荷调节剂、10份的酞青蓝、4份的二甲基二氯硅烷和10份的六甲基二硅氮烷,待用。
先将聚酯树脂、聚丙烯蜡、电荷调节剂和酞青蓝倒入混炼机中,经均匀混合,制成混合料;
再将上述混合料投入挤塑机中,在150℃的温度下将混合料剂出,压制成片;然后,将片状混合料冷却至45℃,并粉碎成碎片;
之后,用粉碎机将上述碎片粉碎成粒径为50μm的碎粉;
之后,用压力为7.5kg/m3压缩空气在流化床粉碎机中对上述碎粉进行气流粉碎并用6000转/分钟的分级机进行分级、用旋风分离器进行分离、用捕集器进行收集,得到粒径为7~9μm的半成品颗粒;
再之后,加入二甲基二氯硅烷和六甲基二硅氮烷,用950转/分钟的混炼机混合4分钟,使其流动性大于20%;
最后,用250目筛网过筛,制成彩色复印机用青色碳粉。
其中:聚酯树脂是按照对苯二甲酸酯∶间苯二甲酸酯=2∶8的比例反应而成的二元共聚物;电荷调节剂是金属水杨酸铬合物。

Claims (2)

1.彩色复印机用青色碳粉,其特征在于由以下重量份数的原材料组成:
聚酯树脂80~90份;
聚丙烯蜡5~10份;
电荷调节剂3~9份;
酞青蓝7~10份;
二甲基二氯硅烷2~4份;
六甲基二硅氮烷7~10份;
其中:所说的聚酯树脂是按照对苯二甲酸酯∶间苯二甲酸酯=2∶8的比例反应而成的二元共聚物,所说的电荷调节剂是金属水杨酸铬合物或金属偶氮铬合物。
2.根据权利要求1所述彩色复印机用红色碳粉的制备方法,其特征在于依次包括以下步骤:
(1)先将聚酯树脂、聚丙烯蜡、酞青蓝和电荷调节剂倒入混炼机中,经均匀混合,制成混合料;
(2)再将上述混合料投入挤塑机中,在90~150℃的温度下将混合料挤出压制成片;然后,
将片状混合料冷却至40~45℃并粉碎成碎片;
(3)之后,用粉碎机将上述碎片粉碎成粒径为30~50μm的碎粉;
(4)之后,用粉碎机对上述碎粉进行进一步粉碎,并依次进行分级、分离、收集,得到粒径为7~9μm的半成品颗粒;
(5)再之后,加入二甲基二氯硅烷和六甲基二硅氮烷,用850~950转/分钟的混炼机混合3~4分钟,使其流动性大于20%;
(6)最后,用200~250目筛网过筛,制成彩色复印机用青色碳粉。
CNB2006100411235A 2006-08-02 2006-08-02 彩色复印机用青色碳粉及其制备方法 Active CN100437362C (zh)