WO2025258207A1 - 溶融亜鉛めっき鋼板及びその製造方法 - Google Patents

溶融亜鉛めっき鋼板及びその製造方法

Info

Publication number
WO2025258207A1
WO2025258207A1 PCT/JP2025/014247 JP2025014247W WO2025258207A1 WO 2025258207 A1 WO2025258207 A1 WO 2025258207A1 JP 2025014247 W JP2025014247 W JP 2025014247W WO 2025258207 A1 WO2025258207 A1 WO 2025258207A1
Authority
WO
WIPO (PCT)
Prior art keywords
steel sheet
less
hot
dip galvanized
galvanized steel
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
PCT/JP2025/014247
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
魁人 多川
一輝 遠藤
裕美 吉冨
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
JFE Steel Corp
Original Assignee
JFE Steel Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by JFE Steel Corp filed Critical JFE Steel Corp
Priority to JP2025549621A priority Critical patent/JP7786653B1/ja
Publication of WO2025258207A1 publication Critical patent/WO2025258207A1/ja
Pending legal-status Critical Current
Anticipated expiration legal-status Critical

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D9/00—Heat treatment, e.g. annealing, hardening, quenching or tempering, adapted for particular articles; Furnaces therefor
    • C21D9/46—Heat treatment, e.g. annealing, hardening, quenching or tempering, adapted for particular articles; Furnaces therefor for sheet metals
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/06—Ferrous alloys, e.g. steel alloys containing aluminium
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/60—Ferrous alloys, e.g. steel alloys containing lead, selenium, tellurium, or antimony, or more than 0.04% by weight of sulfur
    • C—CHEMISTRY; METALLURGY
    • C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
    • C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
    • C23C2/00—Hot-dipping or immersion processes for applying the coating material in the molten state without affecting the shape; Apparatus therefor
    • C23C2/04—Hot-dipping or immersion processes for applying the coating material in the molten state without affecting the shape; Apparatus therefor characterised by the coating material
    • C23C2/06—Zinc or cadmium or alloys based thereon
    • C—CHEMISTRY; METALLURGY
    • C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
    • C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
    • C23C2/00—Hot-dipping or immersion processes for applying the coating material in the molten state without affecting the shape; Apparatus therefor
    • C23C2/26—After-treatment
    • C23C2/28—Thermal after-treatment, e.g. treatment in oil bath
    • C—CHEMISTRY; METALLURGY
    • C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
    • C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
    • C23C2/00—Hot-dipping or immersion processes for applying the coating material in the molten state without affecting the shape; Apparatus therefor
    • C23C2/34—Hot-dipping or immersion processes for applying the coating material in the molten state without affecting the shape; Apparatus therefor characterised by the shape of the material to be treated
    • C23C2/36—Elongated material
    • C23C2/40—Plates; Strips

Definitions

  • the present invention relates to hot-dip galvanized steel sheets and their manufacturing methods.
  • Patent Document 1 discloses a high-strength steel sheet with a tensile strength of 1180 MPa or more, a soft surface layer with a thickness of more than 10 ⁇ m, and a soft surface layer containing carbides at a predetermined number density.
  • Patent Document 2 discloses a hot-dip galvanized steel sheet with a tensile strength of 1180 MPa or more, in which the thickness of the soft surface layer is controlled and bendability is improved by reducing the amount of low-temperature diffusible hydrogen in the steel.
  • Patent Document 1 it is necessary to control the amount of hydrogen in the steel from the perspective of hydrogen embrittlement resistance, and there is no consideration of balancing this with the properties of the welded joint, leaving room for improvement. Furthermore, to ensure dimensional accuracy, it is necessary to control TS and YS, but there is no disclosure about YS in Patent Document 1, leaving room for improvement. In Patent Document 2, there is no consideration of the properties of the welded joint, leaving room for improvement.
  • the present invention aims to provide a hot-dip galvanized steel sheet having a TS of 1700 MPa or more and a YS of 1250 MPa or more, and excellent formability, corona bond peel strength, and resistance to delayed peeling of welded joints, as well as a manufacturing method thereof.
  • formability refers to hole expandability and bendability.
  • the substrate steel sheet has a predetermined chemical composition, a steel structure containing a certain amount of tempered martensite, and a microstructure containing ferrite and/or retained austenite, which allows a YS of 1250 MPa or more to be achieved, and also allows a high TS and excellent bendability to be achieved.
  • the C content in the surface layer of the base steel sheet 0.250% or less and the value obtained by dividing the C content in the surface layer of the steel sheet by the C content of the entire steel sheet less than 0.85, a soft surface layer is formed and excellent peel strength is obtained in the corona bond.
  • High hole expandability can be achieved by reducing the amount of hydrogen trapped in specific hydrogen trapping sites in the base steel sheet, and further reducing the amount to a level appropriate for the hardness of the steel sheet surface layer can suppress crack propagation to the nugget, thereby achieving excellent resistance to delayed peeling of the weld.
  • the gist of the present invention is as follows:
  • a steel sheet having a base steel sheet and a hot-dip galvanized layer formed on the surface of the base steel sheet comprises, in mass%, C: more than 0.250% and not more than 0.400%; Si: 0.01% or more and 2.50% or less, Mn: 0.10% or more and 5.00% or less, P: 0.100% or less, S: 0.0200% or less, Al: 0.100% or less, A component composition containing N: 0.0100% or less and O: 0.0100% or less, with the balance being Fe and unavoidable impurities;
  • the area ratio of tempered martensite is 60.0% or more,
  • the area ratio of quenched martensite is 10.0% or less, and a steel structure in which the area fraction of ferrite is 30.0% or less and the volume fraction of retained austenite is 10.0% or less
  • the C content in the surface layer of the substrate steel sheet is 0.250% or less, a value obtained by dividing the
  • the component composition further includes, in mass%, Ti: 0.200% or less, Nb: 0.200% or less, V: 0.200% or less, Ta: 0.100% or less, W: 0.100% or less, B: 0.0100% or less, Cr: 1.000% or less, Mo: 1.000% or less, Ni: 1.000% or less, Co: 0.500% or less, Cu: 1.00% or less, Sn: 0.200% or less, Sb: 0.200% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, REM: 0.0100% or less, Zr: 0.1000% or less, Te: 0.1000% or less,
  • the present invention provides a hot-dip galvanized steel sheet and its manufacturing method that has a TS of 1700 MPa or more and a YS of 1250 MPa or more, and that is excellent in formability, corona bond peel strength, and resistance to delayed peeling of welded joints.
  • FIG. 2 is a schematic diagram of a tensile test piece used in evaluating the peel strength of a corona bond in the examples of the present invention.
  • 1A and 1B are a top view and a side view, respectively, of a welded joint used in evaluating delayed peeling resistance in an example of the present invention.
  • base steel plate First, the chemical composition of the base steel sheet of the hot-dip galvanized steel sheet according to one embodiment of the present invention will be described. Note that “%” representing the content of component elements means “mass %” unless otherwise specified.
  • Carbon (C) is one of the important basic components of steel, and in the present invention, it is an important element that affects the thermal stress (TS), bendability, and weld corona bond peel strength. If the C content is 0.250% or less, the hardness of quenched martensite and tempered martensite decreases, making it difficult to achieve the desired TS. Therefore, the C content is set to more than 0.250%, preferably 0.255% or more, and more preferably 0.260% or more. On the other hand, if the C content exceeds 0.400%, the quenched martensite and tempered martensite become embrittled, making it difficult to achieve the desired bendability.
  • the C content is set to 0.400% or less, preferably 0.380% or less, and more preferably 0.370% or less.
  • Si 0.01% or more and 2.50% or less
  • Si is one of the important basic components of steel.
  • Si suppresses carbide formation during annealing and promotes the formation of retained austenite, thereby affecting the volume fraction of retained austenite.
  • Si reduces the number of void initiation sites during bending, making it an effective element for improving bendability.
  • the Si content is set to 0.01% or more, preferably 0.20% or more, and more preferably 0.25% or more.
  • the Si content is set to 2.50% or less, preferably 2.00% or less, and more preferably 1.50% or less.
  • Mn 0.10% or more and 5.00% or less
  • Mn is one of the important basic components of steel.
  • it is an important element that affects the area fraction of tempered martensite, the area fraction of ferrite, and the volume fraction of retained austenite.
  • Mn is an important element that improves the hardenability of steel and suppresses ferrite transformation during cooling after annealing, thereby increasing the area fraction of tempered martensite.
  • the Mn content is set to 0.10% or more, preferably 1.00% or more, and more preferably 2.00% or more.
  • the Mn content is set to 5.00% or less, preferably 4.00% or less, and more preferably 3.50% or less.
  • the P content is set to 0.100% or less, and preferably 0.070% or less.
  • the P content is preferably set to 0.001% or more.
  • S 0.0200% or less
  • S exists as sulfide and reduces the ultimate deformability of steel, so if S is contained in excess, hole expandability and bendability will decrease. Therefore, the S content is set to 0.0200% or less, and preferably 0.0050% or less. Although there is no particular lower limit for the S content, due to constraints on production technology, the S content is preferably set to 0.0001% or more.
  • Al 0.100% or less
  • the Al content is set to 0.100% or less, and preferably 0.050% or less.
  • the Al content is preferably set to 0.001% or more.
  • N 0.0100% or less
  • N exists as a nitride and reduces the ultimate deformability of the steel sheet, so if N is contained in excess, the hole expandability and bendability will decrease. Therefore, the N content is set to 0.0100% or less, and preferably 0.0050% or less. Although there is no particular lower limit for the N content, due to constraints on production technology, the N content is preferably set to 0.0005% or more.
  • O exists as an oxide and reduces the ultimate deformability of the steel sheet, so if O is contained in excess, the hole expandability and bendability will decrease. Therefore, the O content is set to 0.0100% or less, and preferably 0.0050% or less. There is no particular lower limit for the O content, but due to constraints on production technology, the O content is preferably set to 0.0001% or more.
  • the base steel sheet has a composition containing the above elements with the balance including Fe and unavoidable impurities. Furthermore, the base steel sheet preferably has a composition containing the above elements with the balance consisting of Fe and unavoidable impurities. Examples of unavoidable impurities include Zn, Pb, Sr, Ge, Cs, and As. The inclusion of these impurities is permitted as long as the total content is 0.100% or less.
  • the composition of the high-strength steel plate disclosed herein further includes, by mass%, Ti: 0.200% or less, Nb: 0.200% or less, V: 0.200% or less, Ta: 0.100% or less, W: 0.100% or less, B: 0.0100% or less, Cr: 1.000% or less, Mo: 1.000% or less, Ni: 1.000% or less, Co: 0.500% or less, C It may contain at least one element selected from the group consisting of u: 1.00% or less, Sn: 0.200% or less, Sb: 0.200% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, REM: 0.0100% or less, Zr: 0.1000% or less, Te: 0.1000% or less, Hf: 0.100% or less, and Bi: 0.200% or less.
  • Ti 0.200% or less
  • Ti generates large amounts of coarse precipitates or inclusions, reducing the ultimate deformability of the steel sheet, and therefore, if the Ti content exceeds 0.200%, the hole expandability and bendability decrease. Therefore, when Ti is contained, the Ti content is set to 0.200% or less, and preferably 0.100% or less.
  • the Ti content is preferably set to 0.001% or more.
  • Nb generates large amounts of coarse precipitates or inclusions, reducing the ultimate deformability of the steel sheet. Therefore, if the Nb content exceeds 0.200%, the hole expandability and bendability decrease. Therefore, when Nb is contained, the Nb content is set to 0.200% or less, and preferably 0.100% or less. Although there is no particular lower limit for the Nb content, by setting the Nb content to 0.001% or more, fine carbides, nitrides, or carbonitrides are formed during hot rolling or continuous annealing, thereby increasing the strength of the steel sheet and achieving a favorable TS. Therefore, the Nb content is preferably set to 0.001% or more.
  • V 0.200% or less
  • V generates large amounts of coarse precipitates or inclusions, reducing the ultimate deformability of the steel sheet, so if the V content exceeds 0.200%, the hole expandability and bendability decrease. Therefore, when V is contained, the V content is 0.200% or less, and preferably 0.100% or less.
  • the V content is preferably 0.001% or more.
  • Ta or W 0.100% or less
  • the respective contents are set to 0.100% or less, preferably 0.080% or less.
  • the Ta or W content is preferably set to 0.010% or more.
  • the B content is set to 0.0100% or less, and preferably 0.0080% or less. Note that there is no particular lower limit for the B content, but since B is an element that segregates to austenite grain boundaries during annealing and improves hardenability, the B content is preferably set to 0.0003% or more.
  • Co content is set to 0.500% or less, preferably 0.050% or less.
  • the Co content is preferably set to 0.001% or more.
  • the Cu content is set to 1.00% or less, preferably 0.80% or less.
  • the Cu content is preferably set to 0.01% or more.
  • the Sn content is 0.200% or less, preferably 0.100% or less, and more preferably 0.050% or less.
  • the Sn content is preferably 0.001% or more.
  • the Sb content is set to 0.200% or less, preferably 0.100% or less, and more preferably 0.050% or less.
  • the Sb content is preferably set to 0.001% or more.
  • the content of Ca, Mg, or REM is preferably set to 0.0005% or more.
  • the Zr or Te content is set to 0.1000% or less, and preferably 0.0800% or less.
  • the Zr or Te content be 0.0010% or more.
  • Hf 0.100% or less
  • the Hf content is set to 0.100% or less, and preferably 0.080% or less.
  • the Hf content is preferably set to 0.010% or more.
  • Bi content exceeds 0.200%, the amount of coarse precipitates or inclusions increases, reducing the ultimate deformability of the steel sheet, resulting in reduced hole expandability and bendability. Therefore, when Bi is contained, the Bi content is set to 0.200% or less, preferably 0.100% or less. Although there is no particular lower limit for the Bi content, since Bi is an element that reduces segregation, the Bi content is preferably set to 0.001% or more.
  • the steel structure of the substrate steel plate will be explained. Note that the steel structure of the substrate steel plate explained below is that at the 1/4 position in the plate thickness direction of the substrate steel plate (a position corresponding to 1/4 of the plate thickness in the depth direction from the surface of the substrate steel plate).
  • the area fraction of tempered martensite is 60.0% or more, preferably 65.0% or more, more preferably 70.0% or more, and even more preferably 75.0% or more.
  • the area fraction of tempered martensite is preferably 99.0% or less, more preferably 98.0% or less, and even more preferably 97.0% or less.
  • the area fraction of quenched martensite is set to 10.0% or less, preferably 8.0% or less, and more preferably 5.0% or less. Note that there is no particular upper limit for the area fraction of quenched martensite, but from the viewpoint of obtaining a high TS, the area fraction of quenched martensite is preferably 0.1% or more.
  • the area fraction of ferrite in the steel structure of the base steel sheet is 30.0% or less, the desired TS, excellent hole expandability, and bendability can be achieved. Therefore, the area fraction of ferrite is set to 30.0% or less, and preferably 25.0% or less.
  • the lower limit of the area fraction of ferrite is not particularly limited, and the area fraction of ferrite may be 0.0%.
  • ferrite also includes bainitic ferrite.
  • the area fractions of tempered martensite, quenched martensite, and ferrite can be determined as follows. A sample is cut out so that the observation surface is the thickness cross section (L cross section) parallel to the rolling direction of the steel plate. The observation surface of the cut sample is mirror-polished using diamond paste, and then etched with 3 vol. % nital to reveal the structure. Using a scanning electron microscope (SEM), 10 fields of view are observed at an observation position 1/4 of the steel plate's thickness at an accelerating voltage of 15 kV and a magnification of 2000x to obtain structure images.
  • SEM scanning electron microscope
  • ferrite including bainitic ferrite
  • quenched martensite is a protruding structure with fine irregularities inside
  • tempered martensite is a recessed structure that contains fine carbides.
  • volume fraction of retained austenite 10.0% or less
  • the volume fraction of retained austenite in the steel structure of the substrate steel sheet is 10.0% or less
  • the amount of hydrogen in the steel of the substrate steel sheet can be reduced, and excellent hole expandability and resistance to delayed disbonding of welded joints can be obtained. Therefore, the volume fraction of retained austenite is set to 10.0% or less, preferably 9.0% or less, more preferably 8.0% or less, and even more preferably 7.0% or less.
  • the volume fraction of retained austenite can be considered to be the same as its area fraction.
  • the volume fraction of retained austenite is measured as follows. After grinding the sample so that the observation surface is located 1/4 of the sheet thickness from the surface of the substrate steel sheet, it is further polished by 0.1 mm using chemical polishing. Using an X-ray diffraction device with a Co K ⁇ radiation source, the integrated reflection intensity of the (200), (220), and (311) planes of fcc iron (austenite) and the (200), (211), and (220) planes of bcc iron is measured for the observation surface. The volume fraction of austenite can be calculated from the intensity ratio of the integrated reflection intensity from each plane of fcc iron to the integrated reflection intensity from each plane of bcc iron.
  • the area ratio of the remaining structure other than tempered martensite, quenched martensite, ferrite, and retained austenite is preferably 5.0% or less.
  • the remaining structure include other known structures of steel sheets, such as pearlite, cementite, and metastable carbides (e.g., epsilon ( ⁇ ) carbide, eta ( ⁇ ) carbide, and chi ( ⁇ ) carbide).
  • the remaining structure can be identified, for example, by observation using a SEM.
  • the area ratio of the remaining structure can be calculated by the following formula (2).
  • [Area fraction of remaining structure (%)] 100 - [Area fraction of tempered martensite (%)] - [Area fraction of quenched martensite (%)] - [Area fraction of ferrite (%)] - [Volume fraction of retained austenite (%)] ...
  • Forming a soft layer on the surface of the substrate steel sheet and reducing the surface layer hardness improves the toughness of the corona bond and increases the peel strength of the corona bond.
  • the surface layer hardness can be reduced by reducing the C content in the surface layer. Therefore, the C content in the surface layer of the substrate steel sheet is set to 0.250% or less, and preferably 0.230% or less.
  • the C content in the surface layer of the substrate steel sheet is set to 0.010% or more.
  • the carbon content in the surface layer of the substrate steel sheet can be determined as follows. A 20 mm square sample is taken from the substrate steel sheet to be measured. The sample is measured using discharge optical emission spectroscopy (GDS) with a 4 mm diameter anode, a high-frequency discharge pressure of 300 MPa, a high-frequency output of 35 W, a pulse frequency of 100 Hz, and a measurement time of 0 to 6000 seconds. Zn derived from the plating is detected approximately 5 ⁇ m from the surface layer. The carbon content in the surface layer of the substrate steel sheet is determined as the carbon content at a depth 10 ⁇ m in the thickness direction of the substrate steel sheet from the depth where the Zn concentration is 0.0 mass%. The carbon content of the entire substrate steel sheet is the carbon content in the chemical composition of the substrate steel sheet described above, and is equivalent to the carbon content of the steel slab used.
  • GDS discharge optical emission spectroscopy
  • the bond energy with the hydrogen trapping site of the base steel sheet is low, hydrogen is easily desorbed by diffusion and does not affect the delayed disbonding resistance properties of the weld, so the bond energy is preferably 15 kJ/mol or more.
  • hydrogen with high bond energy is less likely to desorb from the trapping site and similarly does not affect the delayed disbonding resistance properties of the weld, so the bond energy is preferably 80 kJ/mol or less.
  • the average Vickers hardness HvS of the surface layer of the substrate steel sheet is preferably 100 or more, since an excessive decrease in the strength of the surface layer of the steel sheet results in a decrease in the strength of the entire steel sheet.
  • the average Vickers hardness HvS of the surface layer of the substrate steel sheet is preferably 550 or less, since an excessive increase in the strength of the surface layer of the steel sheet results in a deterioration in bendability.
  • the obtained activation energy Ea is the sum of the activation energy of hydrogen diffusion in the lattice and the binding energy of hydrogen with the hydrogen trap site. Therefore, the binding energy of hydrogen with the hydrogen trap site can be calculated by subtracting the activation energy of hydrogen diffusion in the lattice, 7.6 kJ/mol, from Ea.
  • the amount of hydrogen in steel [H], where the binding energy with hydrogen trap sites is between 10 kJ/mol and 100 kJ/mol, can be determined as follows: The sample is continuously heated from room temperature to 300°C at a heating rate of 200°C/h, and then cooled to room temperature. During heating, the cumulative amount of hydrogen released from the test piece from room temperature to 210°C is measured and used as the amount of hydrogen in steel [H].
  • the average Vickers hardness HvS of the surface layer of the substrate steel sheet can be determined as follows. Measurements were made at 20 points at positions 5 ⁇ m in the thickness direction from the surface layer of the substrate steel sheet (the interface between the coating layer and the substrate steel sheet) with a load of 10 g and a load time of 10 seconds. The average value of the measurement results was taken as the average Vickers hardness HvS of the surface layer of the substrate steel sheet.
  • the hot-dip galvanized layer includes an alloyed hot-dip galvanized layer (a plating layer obtained by subjecting a hot-dip galvanized layer to an alloying treatment).
  • the hot-dip galvanized layer is provided on both surfaces of the substrate steel sheet.
  • the chemical composition of the hot-dip galvanized layer is not particularly limited and may be any common one.
  • it may contain 20% by mass or less of Fe, 0.001% by mass or more and 1.0% by mass or less of Al, and a total of 0.0% by mass or more and 3.5% by mass or less of at least one element selected from the group consisting of Pb, Sb, Si, Sn, Mg, Mn, Ni, Cr, Co, Ca, Cu, Li, Ti, Be, Bi, and REM, with the remainder consisting of Zn and unavoidable impurities.
  • the Fe content of the hot-dip galvanized layer may be less than 7% by mass.
  • the Fe content of the hot-dip galvanized layer is preferably 7% by mass or more and 15% by mass or less, and more preferably 8% by mass or more and 13% by mass or less.
  • the plating amount per side is not particularly limited, but is preferably 20 to 80 g/ m2 .
  • the thickness of the hot-dip galvanized steel sheet is not particularly limited, but is usually between 0.3 mm and 2.8 mm.
  • TS Tensile strength
  • the hot-dip galvanized steel sheet has a TS of 1700 MPa or more.
  • TS can be determined as follows: A JIS No. 5 test piece is taken from the hot-dip galvanized steel sheet so that the tensile direction is perpendicular to the rolling direction. A tensile test is performed in accordance with JIS Z 2241:2011 at a crosshead speed of 1.67 ⁇ 10 -1 mm/s to measure TS.
  • the hot-dip galvanized steel sheet has a YS of 1250 MPa or more.
  • the YS can be determined by the above-mentioned tensile test.
  • Hot-dip galvanized steel sheets have excellent hole expandability.
  • excellent hole expandability means that the hole expandability ratio ⁇ is 30% or more.
  • the hole expandability ratio ⁇ can be determined as follows. A 100 mm ⁇ 100 mm test piece is taken from the hot-dip galvanized steel sheet. A hole expanding test is performed in accordance with JIS Z 2256 (2010). Specifically, a 10 mm diameter hole is punched with a clearance of 12% ⁇ 1%, and a 60° conical punch is pressed into the hole while using a die with an inner diameter of 75 mm and a blank holding force of 9 tons to measure the hole diameter at the crack initiation limit.
  • the hole expandability ratio ⁇ (%) is calculated using the following formula (4), where Df is the hole diameter (mm) at the time of crack initiation and D0 is the initial hole diameter (mm).
  • ⁇ (%) ⁇ (D f - D 0 )/D 0 ⁇ 100 (4)
  • Hot-dip galvanized steel sheets have excellent bendability. Bendability can be evaluated as follows. 24 hours after production, strip-shaped test pieces 30 mm wide and 100 mm long are taken from the hot-dip galvanized steel sheet so that the axial direction of the bending test is parallel to the rolling direction. A 90° V-bend test is performed in accordance with JIS Z 2248:2022 under conditions of an indentation load of 100 kN and a holding time of 5 seconds. The presence or absence of cracks is then determined on the outside of the bent portion using a stereomicroscope, and the minimum bending radius at which no cracks occur is defined as the limit bending radius R. A steel sheet is evaluated as having excellent bendability when it satisfies the condition of limit bending R/t ⁇ 4.50 (t: thickness of the hot-dip galvanized steel sheet) in the 90° V-bend.
  • Hot-dip galvanized steel sheets have excellent corona bond peel strength.
  • Corona bond peel strength can be evaluated as follows. Two 100 mm x 30 mm flat samples are taken from the hot-dip galvanized steel sheet. The flat samples are bent 90° with a curvature of 5 mm at a position 30 mm from the end of the sample, with the bending axis parallel to the short side, to prepare an L-shaped sample. In the L-shaped sample, a square surface approximately 30 mm square serves as the welding surface, and a surface approximately 65 mm x 30 mm serves as the gripping portion for the tensile test.
  • two L-shaped samples 10 are arranged so that their welding surfaces are in contact with each other, and are welded at the center 12 of the welding surface so that the weld has a diameter of 3 mm to 5 mm on each L-shaped sample 10, thereby preparing a tensile test piece 100.
  • a tensile test is performed before hydrogen present inside the weld of the tensile test piece 100 is released, i.e., within 5 minutes after welding.
  • the tensile test conditions are the same as those for the TS evaluation. From the load-displacement graph obtained from the tensile test, the maximum load immediately before a sudden load drop occurs is determined and used as the corona bond peel strength.
  • a corona bond peel strength of 50 N or more is evaluated as excellent.
  • the corona bond peel strength of hot-dip galvanized steel sheet is preferably 55 N or more.
  • Hot-dip galvanized steel sheets have excellent resistance to delayed peeling at welds.
  • the resistance to delayed peeling at welds can be evaluated as follows. Two 100 mm x 30 mm samples were taken from the hot-dip galvanized steel sheet. As shown in Figure 2(b), a welded joint 102 was formed by stacking a sample 20, a spacer 22, and another sample 20 in this order. Two 1.5 mm thick, 30 mm square mild steel sheets were used as the spacers 22. The spacers 22 were sandwiched at both ends of the samples 20, and tack welding was performed. Tack welding was performed at two tack welds 24 shown in Figure 2(a).
  • the center of the tack-welded welded joint 102 was designated as a resistance spot weld 26, and resistance spot welding was performed. After resistance spot welding, the welded joint 102 was left in the air at room temperature (20°C) for at least 24 hours. It is preferable to perform resistance spot welding at room temperature, with the welding electrodes (lower electrode and upper electrode) always water-cooled.
  • the lower and upper electrodes are both DR-type electrodes made of chromium copper, with a tip diameter (tip diameter) of 6 mm and a curvature radius of 40 mm.
  • the pressure is controlled by driving the lower and upper electrodes with a servo motor, and a single-phase alternating current with a frequency of 50 Hz is supplied during current application.
  • the welded joint obtained as described above is processed so that the cross section of the weld can be observed.
  • the cross section of the weld is observed using an SEM. If cracks are found in the nugget at the joint interface, it is determined that delamination has occurred in the weld.
  • the nugget diameter (mm) of the weld is measured, and if the value obtained by dividing the measured nugget diameter by the square root of t (t: thickness of the hot-dip galvanized steel sheet) is 3.5 or greater and no cracks have occurred in the nugget, the weld is evaluated as having excellent resistance to delayed delamination.
  • a steel slab is produced by melting a steel material having the above-described chemical composition.
  • the method for melting the steel material is not particularly limited, and known melting methods such as a converter or an electric furnace can be used.
  • the steel slab is preferably produced by a continuous casting method to prevent macrosegregation, but it can also be produced by an ingot casting method, a thin slab casting method, or the like.
  • the heating temperature of the steel slab is preferably 1100°C or higher and 1300°C or lower. Precipitates present during the heating stage of the steel slab exist as coarse precipitates in the final base steel sheet and do not contribute to strength, so it is preferable to redissolve the Ti and Nb-based precipitates precipitated during casting. Therefore, the heating temperature of the steel slab is preferably 1100°C or higher, more preferably 1150°C or higher. Furthermore, from the viewpoint of scaling off defects such as bubbles and segregations on the surface of the slab, reducing cracks and irregularities on the steel sheet surface, and achieving a smooth steel sheet surface, the heating temperature of the steel slab is preferably 1100°C or higher.
  • the heating temperature of the steel slab exceeds 1300°C, the amount of oxidation increases, resulting in increased scale loss. Therefore, the heating temperature of the steel slab is preferably 1300°C or lower, more preferably 1250°C or lower. Furthermore, steel slabs are made into sheet bars by rough rolling under normal conditions, but when the heating temperature is set low, it is preferable to heat the sheet bar using a bar heater or the like before finish rolling in order to prevent problems during hot rolling.
  • Hot rolling delivery temperature of hot rolling 750°C or higher and 1000°C or lower
  • the heated steel slab is hot-rolled to produce a hot-rolled steel sheet.
  • Hot rolling includes rough rolling and finish rolling.
  • the finish rolling exit temperature exceeds 1000°C, the amount of oxide (scale) generated increases rapidly, the interface between the base steel and the oxide becomes rough, and the surface quality after pickling or cold rolling tends to deteriorate.
  • the presence of residual hot-rolled scale after pickling has a negative effect on bendability.
  • the crystal grain size becomes excessively coarse, which may cause surface roughness of the pressed product during processing. Therefore, the finish rolling exit temperature is set to 1000°C or less, and preferably 950°C or less.
  • the hot-rolled steel sheet after hot rolling is coiled. If the coiling temperature of the hot-rolled steel sheet exceeds 750°C, scale is formed on the surface layer of the hot-rolled steel sheet, causing excessive surface decarburization during the subsequent heat treatment process, reducing the surface hardness and making it difficult to obtain sufficient corona bond peel strength. Therefore, the coiling temperature of the hot-rolled steel sheet is set to 750°C or less, and preferably 650°C or less.
  • the coiling temperature of the hot-rolled steel sheet is set to 300°C or more, and preferably 400°C or more. The coiling temperature is based on the temperature of the surface of the hot-rolled steel sheet.
  • rough-rolled sheets may be joined together during hot rolling, and continuous finish rolling may be performed.
  • the rough-rolled sheet (sheet bar) may be temporarily wound before finish rolling.
  • some or all of the finish rolling may be performed as lubricated rolling.
  • Lubricated rolling is also preferable from the perspective of uniforming the steel sheet shape and material properties.
  • the coefficient of friction during lubricated rolling is preferably in the range of 0.10 to 0.25.
  • the hot-rolled sheet is then pickled.
  • Pickling removes oxides from the steel sheet surface, making it important for ensuring good chemical conversion treatment properties and plating quality in the final hot-dip galvanized steel sheet product. Pickling may be performed once or in multiple steps.
  • the hot-rolled steel sheet is subjected to cold rolling to obtain a cold-rolled steel sheet.
  • the rolling method is not particularly limited, it is preferable to perform cold rolling by multi-pass rolling, which requires two or more passes, such as tandem multi-stand rolling or reverse rolling, since this allows strain to be uniformly and efficiently introduced to obtain a uniform structure. If the cold-rolling reduction ratio exceeds 60.0%, the grain size of austenite formed in the subsequent annealing step becomes fine, the stability of austenite improves, and the amount of retained austenite becomes excessive. Therefore, the cold-rolling reduction ratio is set to 60.0% or less, preferably 55.0% or less, and more preferably 50.0% or less.
  • Heating temperature in annealing process ( Ac3 transformation point - 50) ° C. or higher]
  • the cold-rolled steel sheet is annealed. If the heating temperature in the annealing step is less than ( Ac3 transformation point - 50) ° C., the annealing treatment will be performed in the two-phase region of ferrite and austenite, and since a large amount of ferrite will be contained after annealing, it will be difficult to achieve the desired TS, high hole expandability, and high bendability. Therefore, the heating temperature in the annealing step is ( Ac3 transformation point - 50) ° C. or higher, preferably ( Ac3 transformation point - 30) ° C.
  • the heating temperature in the annealing step is preferably 1000 ° C. or lower, more preferably 980 ° C. or lower. Note that the heating temperature in the annealing step is measured based on the temperature of the surface of the cold-rolled steel sheet.
  • the Ac3 transformation point can be determined using the following formula (5).
  • (Ac 3 transformation point) 910-203 ⁇ (%C)+45 ⁇ (%Si)-30 ⁇ (%Mn)-20 ⁇ (%Cu)-15 ⁇ (%Ni)+11 ⁇ (%Cr)+32 ⁇ (%Mo)+104 ⁇ (%V)+400 ⁇ (%Ti)+200 ⁇ (%Al) ...(5)
  • (%C), (%Si), (%Mn), (%Ni), (%Cu), (%Ni) (%Cr), (%Mo), (%V), (%Ti), and (%Al) are the contents (mass%) of elements in the chemical composition of the base steel sheet, and are set to zero if the element is not contained.
  • the time for which the heating temperature is maintained is not particularly limited, but it is preferably between 10 seconds and 600 seconds.
  • the cold-rolled steel sheet is threaded through the snout. If the dew point in the snout is lower than ⁇ 60°C, decarburization from the surface layer of the cold-rolled steel sheet is suppressed and a soft layer is not formed in the surface layer, so the hardness of the surface layer does not decrease, the peel strength of the corona bond decreases, and the delayed peel resistance of the welded portion deteriorates. Therefore, the dew point in the snout is ⁇ 60°C or higher, and ⁇ 50°C or higher is preferable.
  • the dew point in the snout is preferably 30°C or lower, and more preferably 20°C or lower.
  • the cold-rolled steel sheet is subjected to a hot-dip galvanizing treatment to obtain a hot-dip galvanized steel sheet.
  • the annealing, cooling, and galvanizing treatments may be performed continuously in one line (CGL (Continuous Galvanizing Line)), an example of which is described below.
  • CGL Continuous Galvanizing Line
  • the cold-rolled steel sheet is cooled to a temperature range of about 500°C.
  • the cold-rolled steel sheet is passed through the steel strip outlet side of the cooling zone, and further cooled while being moved into the hot-dip galvanizing bath via a snout whose tip is immersed in the hot-dip galvanizing bath.
  • the time from the end of cooling of the cold-rolled steel sheet to the entry of the cold-rolled steel sheet into the hot-dip galvanizing bath is not particularly limited, but is preferably 1 s or more and 300 s or less from the viewpoint of controlling the area ratios of martensite and ferrite.
  • a roll for changing the traveling direction of the cold-rolled steel sheet to enter the snout is provided immediately before the connection part between the cooling zone and the snout, and the cold-rolled steel sheet enters the snout after passing through this roll.
  • the cold-rolled steel sheet is then guided to a hot-dip galvanizing bath through the snout and immersed in the hot-dip galvanizing bath to be subjected to hot-dip galvanizing treatment, thereby producing a plated steel sheet.
  • the cold-rolled steel sheet can be immersed in a hot-dip galvanizing bath at a temperature of 480°C or higher and 500°C or lower.
  • the hot-dip galvanizing bath used in the hot-dip galvanizing process preferably contains an Al content of 0.10% by mass or higher and 0.23% by mass or lower, with the remainder being Zn and unavoidable impurities.
  • the coating weight in the hot-dip galvanizing treatment is preferably 20 to 80 g/m 2 per side (double-sided plating).
  • the coating weight can be adjusted by performing gas wiping or the like after the hot-dip galvanizing treatment.
  • the cold-rolled steel sheet may be subjected to an alloying treatment after hot-dip galvanizing. It is preferable to perform the alloying treatment on the hot-dip galvanized steel sheet after the hot-dip galvanizing treatment and before the vibration holding process described below.
  • the alloying treatment temperature is preferably 460°C or higher, and more preferably 470°C or higher.
  • the alloying treatment temperature is preferably 600°C or lower, and more preferably 560°C or lower.
  • the alloying treatment temperature is based on the surface temperature of the hot-dip galvanized steel sheet.
  • a first cooling step is performed in which the hot-dip galvanized steel sheet is cooled to a cooling stop temperature below the martensitic transformation start temperature. If the cooling stop temperature exceeds the martensitic transformation start temperature, the amount of martensite transformed is small, and the amount of martensite tempered by subsequent reheating is small, making it impossible to obtain the desired amount of tempered martensite. Therefore, the cooling stop temperature in the first cooling step is set to the martensitic transformation start temperature or lower, preferably (martensitic transformation start temperature - 20) °C or lower.
  • the martensitic transformation start temperature (Ms point) can be calculated using the following formula (6).
  • (Martensitic transformation start temperature) 550 - 350 ⁇ (%C) - 40 ⁇ (%Mn) - 10 ⁇ (%Cu) - 17 ⁇ (%Ni) - 20 ⁇ (%Cr) - 10 ⁇ (%Mo) - 35 ⁇ (%V) - 5 ⁇ (%W) + 30 ⁇ (%Al) ...
  • the reheating temperature is preferably above the cooling stop temperature and at least 20°C above the martensitic transformation start temperature.
  • the reheating temperature is set to 450°C or lower, preferably 430°C or lower. Note that the reheating temperature is based on the surface temperature of the hot-dip galvanized steel sheet.
  • a vibration holding step is performed in which the hot-dip galvanized steel sheet is vibrated to a maximum amplitude of 10 nm to 500 ⁇ m and held at the reheating temperature for 2 seconds to 600 seconds.
  • the hot-dip galvanized steel sheet is forcibly vibrated slightly, thereby repeatedly displacing the hot-dip galvanized steel sheet in the sheet thickness direction, i.e., bending deformation. This results in an expansion of the lattice spacing at the surface compared to the center of the thickness of the hot-dip galvanized steel sheet, rather than a uniform expansion of the lattice spacing from the center to the surface.
  • the maximum amplitude of the hot-dip galvanized steel sheet in the vibration holding step is 10 nm or more, preferably 20 nm or more, and more preferably 50 nm or more.
  • the holding time in the vibration holding step is set to 2 seconds or more, and preferably 5 seconds or more.
  • the holding time in the vibration holding step is set to 600 seconds or less, and preferably 550 seconds or less. Note that the holding time is the time during which the quenched martensite is isothermally held at the reheating temperature.
  • the sound pressure on the surface of the steel sheet can be adjusted by adjusting the strength of the sound waves generated by the sound wave emitter and the position of the sound wave emitter (i.e., the distance between the sound wave emitter and the hot-dip galvanized steel sheet).
  • the "sound pressure level on the surface of the hot-dip galvanized steel sheet” can be measured in-line by installing a sound pressure meter near the surface of the hot-dip galvanized steel sheet and directly below the sound wave emitter while it is being threaded.
  • the vibration application time in the vibration holding step is preferably 1 second or more, more preferably 5 seconds or more, and even more preferably 10 seconds or more, from the viewpoint of more sufficiently reducing carbon and hydrogen from the hot-dip galvanized steel sheet.
  • the vibration application time in the vibration holding step is preferably 3600 seconds or less, more preferably 1800 seconds or less, and even more preferably 900 seconds or less, from the viewpoint of not impairing productivity.
  • the vibration application time for the hot-dip galvanized steel sheet means the time during which vibration is applied to each position on the surface of the hot-dip galvanized steel sheet, and when vibration is applied from multiple vibration applying devices, it means the cumulative time of all of the vibrations.
  • a second cooling step is performed in which the hot-dip galvanized steel sheet is cooled to room temperature. It is preferable to continue vibrating the hot-dip galvanized steel sheet even during the second cooling step.
  • the cooling rate in the temperature range of 50°C or more below the martensitic transformation start temperature 15.0°C/s or less (preferred conditions)
  • the transformation to the martensite phase which has low amounts of carbon and hydrogen dissolved therein, can be favorably promoted.
  • the diffusion of carbon and hydrogen can be favorably promoted while generating vibration, i.e., displacement in the thickness direction of the hot-dip galvanized steel sheet. This reduces the C content in the surface layer and the amount of hydrogen in the steel, thereby improving hole expandability and corona bond peel strength.
  • the cooling rate is preferably 15.0°C/s or less, more preferably 12.5°C/s or less, and even more preferably 10.0°C/s or less. While there is no particular lower limit for the cooling rate, due to production technology constraints, the cooling rate is preferably 1.0°C/s or more, more preferably 2.0°C/s or more.
  • the cooling rate is based on the surface temperature of the hot-dip galvanized steel sheet. In addition, as a method for cooling the hot-dip galvanized steel sheet in a temperature range of 50° C. or more below the martensitic transformation start temperature, gas jet cooling, mist cooling, water cooling, air cooling, etc. can be applied.
  • the resulting sheet bar was finish-rolled, coiled, and cooled to obtain a hot-rolled steel sheet.
  • the resulting hot-rolled steel sheet was pickled and then cold-rolled to obtain a cold-rolled steel sheet with a thickness of 1.4 mm.
  • the resulting cold-rolled steel sheet was then annealed and hot-dip galvanized to obtain a hot-dip galvanized steel sheet with a hot-dip galvanized layer on both sides.
  • the resulting hot-dip galvanized steel sheet was cooled while being vibrated by applying ultrasonic waves.
  • the resulting hot-dip galvanized steel sheet was cooled while being vibrated by periodically applying electromagnetic force from an electromagnet.
  • No. 7 the resulting hot-dip galvanized steel sheet was cooled while being vibrated by periodically applying electromagnetic force from an electromagnet.
  • Table 2 shows the manufacturing conditions for each example.
  • "GI” indicates that only hot-dip galvanizing was performed, and "GA” indicates that both hot-dip galvanizing and alloying were performed. Vibration was applied simultaneously with the start of cooling of the hot-dip galvanized steel sheet.
  • a hot-dip galvanizing bath containing 0.20 mass% Al, with the balance being Zn and unavoidable impurities was used as the plating bath.
  • a hot-dip galvanizing bath containing 0.14 mass% Al, with the balance being Zn and unavoidable impurities was used.
  • the plating bath temperature was 470°C in both cases.
  • the coating weight was approximately 45 to 72 g/m 2 per side (double-sided plating) in the GI example, and approximately 45 g/m 2 per side (double-sided plating) in the GA example.
  • the alloying treatment temperature was approximately 550°C.
  • the composition of the resulting hot-dip galvanized layer was Fe: 0.1-1.0% by mass, Al: 0.2-1.0% by mass, with the balance being Zn and unavoidable impurities.
  • the composition of the alloyed hot-dip galvanized layer was Fe: 7-15% by mass, Al: 0.1-1.0% by mass, with the balance being Zn and unavoidable impurities.
  • the structure of the obtained hot-dip galvanized steel sheets was identified at a position 1/4 of the sheet thickness of the substrate steel sheet using the method described above. Furthermore, the C content in the surface layer of the substrate steel sheet, the value obtained by dividing the C content by the total C content of the substrate steel sheet, the amount of hydrogen in the steel [H], and the average Vickers hardness of the surface layer of the substrate steel sheet were evaluated. The evaluation results are shown in Table 3.
  • the chemical composition of the substrate steel sheets of the obtained hot-dip galvanized steel sheets was substantially the same as the chemical composition at the steel slab stage. In other words, all of the conforming steels were within the chemical composition range described above in accordance with the embodiment, while all of the comparative steels were outside the chemical composition range described above in accordance with the embodiment.
  • the inventive examples had a TS of 1700 MPa or more and a YS of 1250 MPa or more, and were excellent in hole expansion, bendability, corona bond peel strength, and weld delayed peel resistance.
  • the comparative examples were inferior in one or more of TS, bendability, corona bond peel strength, and weld delayed peel resistance.
  • the present invention provides a hot-dip galvanized steel sheet and a manufacturing method thereof that has a TS of 1700 MPa or more and a YS of 1250 MPa or more, and that is excellent in formability, corona bond peel strength, and resistance to delayed peeling of welded joints.
  • the hot-dip galvanized steel sheet obtained by the present invention can be applied to, for example, automotive structural components, thereby reducing the vehicle body weight and improving fuel economy, making it extremely valuable in industry.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Engineering & Computer Science (AREA)
  • Materials Engineering (AREA)
  • Mechanical Engineering (AREA)
  • Metallurgy (AREA)
  • Organic Chemistry (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Physics & Mathematics (AREA)
  • Thermal Sciences (AREA)
  • Crystallography & Structural Chemistry (AREA)
  • Oil, Petroleum & Natural Gas (AREA)
  • Heat Treatment Of Sheet Steel (AREA)
PCT/JP2025/014247 2024-06-11 2025-04-09 溶融亜鉛めっき鋼板及びその製造方法 Pending WO2025258207A1 (ja)

Priority Applications (1)

Application Number Priority Date Filing Date Title
JP2025549621A JP7786653B1 (ja) 2024-06-11 2025-04-09 溶融亜鉛めっき鋼板及びその製造方法

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2024-094702 2024-06-11
JP2024094702 2024-06-11

Publications (1)

Publication Number Publication Date
WO2025258207A1 true WO2025258207A1 (ja) 2025-12-18

Family

ID=98050836

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2025/014247 Pending WO2025258207A1 (ja) 2024-06-11 2025-04-09 溶融亜鉛めっき鋼板及びその製造方法

Country Status (2)

Country Link
JP (1) JP7786653B1 (cg-RX-API-DMAC7.html)
WO (1) WO2025258207A1 (cg-RX-API-DMAC7.html)

Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2022014131A1 (ja) * 2020-07-14 2022-01-20 Jfeスチール株式会社 連続焼鈍装置及び連続溶融亜鉛めっき装置、並びに鋼板の製造方法
WO2023286440A1 (ja) * 2021-07-14 2023-01-19 Jfeスチール株式会社 連続焼鈍装置及び連続溶融亜鉛めっき装置、並びに鋼板の製造方法
WO2023113387A1 (ko) * 2021-12-14 2023-06-22 주식회사 포스코 굽힘 특성이 우수한 초고강도 강판 및 이의 제조방법
WO2023162891A1 (ja) * 2022-02-25 2023-08-31 日本製鉄株式会社 鋼板、および鋼板の製造方法
WO2024029145A1 (ja) * 2022-08-03 2024-02-08 日本製鉄株式会社 鋼板

Patent Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2022014131A1 (ja) * 2020-07-14 2022-01-20 Jfeスチール株式会社 連続焼鈍装置及び連続溶融亜鉛めっき装置、並びに鋼板の製造方法
WO2023286440A1 (ja) * 2021-07-14 2023-01-19 Jfeスチール株式会社 連続焼鈍装置及び連続溶融亜鉛めっき装置、並びに鋼板の製造方法
WO2023113387A1 (ko) * 2021-12-14 2023-06-22 주식회사 포스코 굽힘 특성이 우수한 초고강도 강판 및 이의 제조방법
WO2023162891A1 (ja) * 2022-02-25 2023-08-31 日本製鉄株式会社 鋼板、および鋼板の製造方法
WO2024029145A1 (ja) * 2022-08-03 2024-02-08 日本製鉄株式会社 鋼板

Also Published As

Publication number Publication date
JPWO2025258207A1 (cg-RX-API-DMAC7.html) 2025-12-18
JP7786653B1 (ja) 2025-12-16

Similar Documents

Publication Publication Date Title
JP7001202B1 (ja) 鋼板及び部材
KR102852856B1 (ko) 강판, 부재 및 그들의 제조 방법
JP7606111B2 (ja) 鋼板及びその製造方法
JP6787535B1 (ja) 高強度鋼板およびその製造方法
JP6187710B2 (ja) 合金化溶融亜鉛めっき鋼板およびその製造方法
CN114008234A (zh) 高强度钢板及其制造方法
JP5058508B2 (ja) 低降伏比型高ヤング率鋼板、溶融亜鉛めっき鋼板、合金化溶融亜鉛めっき鋼板及び鋼管、並びにそれらの製造方法
US11643700B2 (en) High-strength steel sheet and production method thereof
JP7673874B1 (ja) 高強度鋼板、高強度めっき鋼板及びそれらの製造方法、ならびに、部材
JP7619483B2 (ja) 亜鉛めっき鋼板、部材およびそれらの製造方法
WO2022004818A1 (ja) 鋼板、部材及びそれらの製造方法
CN114585765B (zh) 高强度钢板及其制造方法
WO2023188539A1 (ja) 鋼板、部材およびそれらの製造方法
JP4964488B2 (ja) プレス成形性の良好な高強度高ヤング率鋼板、溶融亜鉛めっき鋼板、合金化溶融亜鉛めっき鋼板及び鋼管、並びにそれらの製造方法
JP7176666B1 (ja) クラッド鋼板および部材、ならびに、それらの製造方法
JP5609793B2 (ja) 溶融めっき冷延鋼板の製造方法
JP7786653B1 (ja) 溶融亜鉛めっき鋼板及びその製造方法
JP7786652B1 (ja) 溶融亜鉛めっき鋼板及びその製造方法
WO2023218730A1 (ja) 鋼板、部材およびそれらの製造方法
CN114585758B (zh) 高强度钢板和碰撞吸收构件以及高强度钢板的制造方法
WO2025258205A1 (ja) 溶融亜鉛めっき鋼板及びその製造方法
WO2025258204A1 (ja) 溶融亜鉛めっき鋼板及びその製造方法
JP7673875B1 (ja) 高強度鋼板、高強度めっき鋼板及びそれらの製造方法並びに部材
JP7613635B2 (ja) 亜鉛めっき鋼板、部材及びそれらの製造方法
JP7711775B2 (ja) 溶融亜鉛めっき鋼板、溶融亜鉛めっき鋼板を用いてなる部材、部材からなる自動車の骨格構造部品又は自動車の補強部品、ならびに溶融亜鉛めっき鋼板及び部材の製造方法

Legal Events

Date Code Title Description
ENP Entry into the national phase

Ref document number: 2025549621

Country of ref document: JP

Kind code of ref document: A

WWE Wipo information: entry into national phase

Ref document number: 2025549621

Country of ref document: JP

121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 25821558

Country of ref document: EP

Kind code of ref document: A1