WO2004092693A2 - Collector for euv light source - Google Patents
Collector for euv light source Download PDFInfo
- Publication number
- WO2004092693A2 WO2004092693A2 PCT/US2004/010972 US2004010972W WO2004092693A2 WO 2004092693 A2 WO2004092693 A2 WO 2004092693A2 US 2004010972 W US2004010972 W US 2004010972W WO 2004092693 A2 WO2004092693 A2 WO 2004092693A2
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- ofthe
- sputtering
- reflecting surface
- rate
- time
- Prior art date
Abstract
Description
Claims