RU2792211C1 - Method for obtaining matted base material with an anti-fingerprint coating - Google Patents

Method for obtaining matted base material with an anti-fingerprint coating Download PDF

Info

Publication number
RU2792211C1
RU2792211C1 RU2021132820A RU2021132820A RU2792211C1 RU 2792211 C1 RU2792211 C1 RU 2792211C1 RU 2021132820 A RU2021132820 A RU 2021132820A RU 2021132820 A RU2021132820 A RU 2021132820A RU 2792211 C1 RU2792211 C1 RU 2792211C1
Authority
RU
Russia
Prior art keywords
layer
formaldehyde resin
applying
resin powder
powdered
Prior art date
Application number
RU2021132820A
Other languages
Russian (ru)
Inventor
Норберт КАЛЬВА
Йоахим ХАШ
Бернд ШТИВЕ
Original Assignee
Флуринг Текнолоджис Лтд.
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Флуринг Текнолоджис Лтд. filed Critical Флуринг Текнолоджис Лтд.
Application granted granted Critical
Publication of RU2792211C1 publication Critical patent/RU2792211C1/en

Abstract

FIELD: manufacture of floor coverings, furniture; materials for wall and ceiling cladding.
SUBSTANCE: method for producing a base material provided with a frosted anti-fingerprint coating includes applying a layer of powdered formaldehyde resin to at least one side of the base material and melting it. Then, a dispersion material containing acrylate is applied to the melted formaldehyde resin layer. The resulting layered structure is dried and cured. The base material is a layer of paper or a board based on wood material. A layer of paper and a plate are also proposed.
EFFECT: group of inventions makes it possible to reduce the gloss level of the material and increase its wear resistance.
25 cl, 5 dwg

Description

Настоящее изобретение относится к способу получения матированного материала-основы, снабженного покрытием, препятствующим сохранению отпечатков пальцев, в частности плиты на основе древесного материала, снабженной узором, или слоя бумаги.The present invention relates to a method for producing a matt base material provided with an anti-fingerprint coating, in particular a patterned wood based board or paper layer.

Применение плит на основе древесного материала в мебельной промышленности в качестве напольных покрытий или также для облицовки стен и потолков требует обработки или улучшения поверхности плит на основе древесного материала. В случае указанных областей применения плиты на основе древесного материала обычно покрываются пропитанной декоративной бумагой. Нет никаких ограничений на разнообразие декоративных бумаг с различным рисунком, поэтому плиты на основе древесного материала можно приобрести с множеством различных узоров, таких как, например, узоры под камень или под дерево. Для повышения устойчивости к истиранию на декоративную бумагу наносятся декоративные накладки. Декоративные накладки представляют собой тонкую прозрачную бумагу, которая, как правило, уже пропитана меламиновой смолой. Также можно приобрести декоративные накладки, в которых уже износостойкие частицы, такие как, например, частицы из корунда, смешиваются со смолой декоративной накладки, чтобы повысить устойчивость к износу слоистого материала или плиты на основе древесного материала.The use of wood-based boards in the furniture industry as floor coverings or also for wall and ceiling cladding requires surface treatment or improvement of the wood-based boards. For these applications, wood-based boards are usually covered with impregnated decorative paper. There is no limit to the variety of decorative papers with different patterns, so wood-based boards can be purchased in many different patterns, such as stone or wood patterns. To increase the resistance to abrasion, decorative overlays are applied to the decorative paper. Decorative overlays are thin transparent paper, which, as a rule, is already impregnated with melamine resin. It is also possible to obtain decorative caps in which already wear-resistant particles, such as for example corundum particles, are mixed with the resin of the trim to increase the wear resistance of the wood-based laminate or board.

В качестве альтернативы применению декоративной бумаги на плитах на основе древесного материала в прошлом была разработана прямая печать на плитах на основе древесного материала, поэтому печать на бумаге и дальнейшее ее ламинирование или прямое нанесение покрытий на плиту на основе древесного материала больше не требуются.As an alternative to the use of decorative paper on wood-based boards, direct printing on wood-based boards was developed in the past, so printing on paper and further laminating or directly coating the wood-based board is no longer required.

Затем на узор, нанесенный посредством прямой печати, наносят несколько слоев жидкой термореактивной смолы, которые могут содержать износостойкие частицы для повышения устойчивости к истиранию. Такой слой термореактивной смолы также называют жидкой декоративной накладкой. Термореактивная смола предпочтительно представляет собой формальдегидсодержащую смолу, в частности меламиноформальдегидную смолу и/или меламиномочевиноформальдегидную смолу. Способ получения описанного слоя жидкой декоративной накладки описан, среди прочего, в EP 2338693 A1. Здесь после очистки поверхности плиты на основе древесного материала на плиту на основе древесного материала происходит нанесение первого верхнего слоя смолы, содержащего частицы из корунда, высушивание этого первого слоя смолы, например, до остаточной влажности от 6 до 10%, последующее нанесение второго слоя смолы, содержащего волокна целлюлозы, на плиту на основе древесного материала, повторное высушивание или подсушивание второго слоя смолы, например, до остаточной влажности от 6 до 10%, нанесение по меньшей мере одного третьего слоя смолы, содержащего частицы из стекла, на плиту на основе древесного материала с последующим подсушиванием третьего слоя смолы, например, также до остаточной влажности от 4 до 8%, и окончательное прессование слоистой структуры под действием давления и температуры. Благодаря применению жидкой декоративной накладки можно отказаться от обычно предусмотренной бумаги-оверлей. Жидкую декоративную накладку можно наносить как на верхнюю сторону, так и на нижнюю сторону плиты на основе древесного материала.The direct-printed pattern is then coated with several layers of liquid thermosetting resin, which may contain wear-resistant particles to improve abrasion resistance. Such a layer of thermosetting resin is also referred to as a liquid decorative overlay. The thermosetting resin is preferably a formaldehyde-containing resin, in particular a melamine-formaldehyde resin and/or a melamine-urea-formaldehyde resin. The method for producing the described layer of liquid decorative overlay is described, inter alia, in EP 2338693 A1. Here, after cleaning the surface of the wood-based board, the first top resin layer containing particles of corundum is applied to the wood-based board, drying this first resin layer, for example, to a residual moisture content of 6 to 10%, then applying the second resin layer, containing cellulose fibers on a board based on wood material, re-drying or drying the second layer of resin, for example, to a residual moisture content of 6 to 10%, applying at least one third layer of resin containing glass particles on a board based on wood material followed by drying the third resin layer, for example also to a residual moisture content of 4 to 8%, and finally pressing the layered structure under pressure and temperature. Thanks to the use of a liquid decorative overlay, the usually provided overlay paper can be dispensed with. The liquid decorative overlay can be applied to both the top side and the bottom side of the wood-based board.

Недостатками применения жидкой декоративной накладки являются затраты на оборудование и связанные с этим требования к пространству. В частности, этапы высушивания после каждого нанесения смолы требуют применения конвекционных сушилок и необходимой обработки отработанного воздуха.The disadvantages of using a liquid decorative overlay are the equipment costs and associated space requirements. In particular, the drying steps after each resin application require the use of convection dryers and the necessary exhaust air treatment.

Помимо вопроса о предоставлении слоя смолы важен также вопрос об оформлении поверхности и структуре поверхности этих продуктов. Это особенно актуально при применении плит на основе древесного материала с нанесенной печатью для внутренней отделки, например мебели, поверхности которой подвергаются сильным нагрузкам при прикосновении, очищении и т.д. При этом часто оценивается особенно негативно, если оформление поверхности и условия освещения позволяют получить особенно хорошую визуальную оценку. Очень точный пример этого - глянцевые фасады на кухнях. В этом случае особенно на этих фасадах при прикосновении часто можно увидеть отпечатки пальцев. В этом случае это особенно касается меламиновых поверхностей. По-видимому, они особенно предрасположены оставлять отпечатки пальцев после прикосновения к ним. Сохранение отпечатков пальцев означает, что поверхности необходимо часто чистить, что отнюдь не желательно. Что касается поверхностей на основе меламина, следует отметить, что они обладают очень высокой механической и химической устойчивостью, что дает им значительные преимущества перед термопластичными пленками или лаками. Кроме того, путем травления пластины для прессования, которые используются при получении покрытых меламиновой смолой плит на основе древесного материала, можно получить практически любой дизайн поверхности. Как уже отмечалось, оформление поверхности является важным аспектом продукции. Как и в случае почти всей продукции, это зависит от модных тенденций. Несколько лет назад глянец был очень популярен для многих продуктов, но сейчас люди больше интересуются матовыми поверхностями. Конечно, на этих поверхностях отпечатки пальцев после прикосновения нежелательны или считаются недостатком.In addition to the issue of providing a layer of resin, the issue of surface design and surface structure of these products is also important. This is especially true when using printed wood-based boards for interior decoration, such as furniture, the surfaces of which are subjected to heavy loads when touched, cleaned, etc. In this case, it is often evaluated especially negatively if the surface design and lighting conditions make it possible to obtain a particularly good visual assessment. A very accurate example of this is glossy fronts in kitchens. In this case, especially on these facades, fingerprints can often be seen when touched. In this case, this applies especially to melamine surfaces. They seem to be particularly prone to leaving fingerprints when touched. The persistence of fingerprints means that surfaces need to be cleaned frequently, which is by no means desirable. With regard to melamine-based surfaces, it should be noted that they have a very high mechanical and chemical resistance, which gives them significant advantages over thermoplastic films or varnishes. In addition, by etching the pressing plate, which is used in the production of melamine resin-coated wood-based boards, almost any surface design can be obtained. As already noted, surface finish is an important aspect of a product. As with almost all products, it depends on fashion trends. A few years ago, gloss was very popular for many products, but now people are more interested in matte surfaces. Of course, on these surfaces, fingerprints after touching are undesirable or considered a disadvantage.

Таким образом, настоящее изобретение основано на технической проблеме обеспечения наличия поверхностей, которые имеют низкую степень блеска и в то же время явно устойчивы к видимости отпечатков пальцев. В то же время этот продукт должен производиться с экономией места и рентабельностью. Высокие значения износа, в частности классы износа от AC4 до AC6, также должны быть достигнуты при одновременно небольшом истирании пластины для прессования.Thus, the present invention is based on the technical problem of providing surfaces that have a low degree of gloss and at the same time are clearly resistant to the visibility of fingerprints. At the same time, this product must be produced in a space-saving and cost-effective way. High wear values, in particular wear classes AC4 to AC6, must also be achieved with at the same time low abrasion of the pressing plate.

Поставленная задача решается в соответствии с настоящим изобретением посредством способа с признаками, указанными в пункте 1 формулы изобретения.The problem is solved in accordance with the present invention by means of a method with the features specified in paragraph 1 of the claims.

Соответственно предоставлен способ получения плиты на основе древесного материала, снабженной узором, при этом способ включает следующие этапы:Accordingly, a method is provided for producing a patterned wood based board, the method comprising the following steps:

- нанесение по меньшей мере одного слоя из по меньшей мере одной порошкообразной смолы на по меньшей мере одну сторону материала-основы;- applying at least one layer of at least one powdered resin on at least one side of the base material;

- плавление по меньшей мере одного нанесенного слоя из порошкообразной смолы;- melting at least one deposited layer of powdered resin;

- нанесение по меньшей мере одного дисперсионного материала, содержащего акрилат, на подплавленный слой смолы и- applying at least one dispersion material containing acrylate to the melted resin layer and

- высушивание и отверждение слоистой структуры.- drying and curing of the layered structure.

Соответственно, предоставляется многостадийный процесс, в котором порошок смолы, например, порошок меламиновой смолы, сначала наносят на материал-основу, например, на слой бумаги или на плиту на основе древесного материала, и обеспечивают загустение или подплавляют. После этого дисперсионный материал на основе акрилата, например с применением щелевого сопла, наносят, высушивают и затем отверждают на поверхности, например, с применением эксимерного излучателя. Эту пропитанную бумагу или эту плиту на основе древесного материала с покрытием можно затем прессовать в прессе с коротким циклом.Accordingly, a multi-step process is provided in which a resin powder, such as melamine resin powder, is first applied to a base material, such as a layer of paper or a wood-based board, and thickened or melted. Thereafter, the acrylate-based dispersion material, for example using a slotted nozzle, is applied, dried and then cured onto the surface, for example using an excimer emitter. This impregnated paper or this coated wood based board can then be pressed in a short cycle press.

Способ согласно настоящему изобретению предоставляет разные преимущества. Таким образом, может быть получена матовая поверхность с единицами блеска менее 10, предпочтительно менее 8, особенно предпочтительно менее 5. Обработанная поверхность обладает свойствами, препятствующими сохранению отпечатков пальцев, и требует минимальных усилий по очистке по сравнению с обычными поверхностями.The method according to the present invention provides various advantages. In this way, a matt surface with gloss units less than 10, preferably less than 8, particularly preferably less than 5 can be obtained. The treated surface has anti-fingerprint properties and requires minimal cleaning effort compared to conventional surfaces.

Кроме того, предоставляется способ получения плит на основе древесного материала, в котором отказываются от использования жидкой смолы для слоистой структуры, а вместо нее используют порошок смолы. При замене порошка смолы жидкой смолой, которая обычно применяется, исключается необходимое для жидких декоративных накладок дорогостоящее высушивание, что снижает стоимость системы, проблемы с отработанным воздухом и требования к пространству. В целом способ согласно настоящему изобретению обеспечивает более гибкую технологию.In addition, there is provided a method for producing boards based on wood material, in which the use of liquid resin for a layered structure is abandoned, and resin powder is used instead. By replacing the resin powder with the liquid resin that is commonly used, the costly drying required for liquid overlays is eliminated, reducing system cost, exhaust air problems, and space requirements. In general, the method according to the present invention provides a more flexible technology.

В одном варианте осуществления способа согласно настоящему изобретению предусмотрено, что дисперсионный материал на основе акрилата содержит отверждаемые излучением лаки, содержащие акрилат. Такие отверждаемые излучением лаки могут быть (мет)акрилатами, такими как, например, сложный-полиэфир(мет)акрилат, простой-полиэфир(мет)акрилат, эпокси(мет)акрилат или уретан(мет)акрилат. Также возможно, что применяемый акрилат или акрилатсодержащий лак присутствует в замещенных или незамещенных мономерах, олигомерах и/или полимерах, в частности в форме мономеров, олигомеров или полимеров акриловой кислоты, простого акрилового эфира и/или сложного эфира акриловой кислоты. При этом присутствие, как определено, двойной связи или ненасыщенной группы в молекуле акрилата важно для способа согласно настоящему изобретению. Полиакрилаты также можно продолжать функционализировать. Подходящие функциональные группы включают, помимо прочего, гидроксильные, амино-, эпоксидные и/или карбоксильные группы. Как уже упоминалось, указанные акрилаты обеспечивают сшивание в присутствии УФ-лучей или электронных лучей в процессе отверждения или высушивания.In one embodiment of the method according to the present invention, it is provided that the acrylate-based dispersion material contains radiation-curable varnishes containing acrylate. Such radiation-curable varnishes can be (meth)acrylates such as, for example, polyester(meth)acrylate, polyether(meth)acrylate, epoxy(meth)acrylate or urethane(meth)acrylate. It is also possible that the acrylate or acrylate-containing lacquer used is present in substituted or unsubstituted monomers, oligomers and/or polymers, in particular in the form of monomers, oligomers or polymers of acrylic acid, acrylic ether and/or acrylic acid ester. The presence, as determined, of a double bond or an unsaturated group in the acrylate molecule is important for the method according to the present invention. Polyacrylates can also be further functionalized. Suitable functional groups include, but are not limited to, hydroxyl, amino, epoxy and/or carboxyl groups. As already mentioned, these acrylates provide crosslinking in the presence of UV rays or electron beams during curing or drying.

Количество наносимого дисперсионного материала, содержащего акрилат, составляет от 30 до 50 фл/м2, предпочтительно от 30 до 40 фл/м2. Содержание твердых частиц дисперсионного материала, содержащего акрилат, составляет от 40 до 60 вес.%, предпочтительно 50 вес.%.The amount of applied dispersion material containing acrylate is from 30 to 50 fl/m 2 , preferably from 30 to 40 fl/m 2 . The solids content of the acrylate-containing dispersion material is 40 to 60% by weight, preferably 50% by weight.

По меньшей мере один дисперсионный материал, содержащий акрилат, после нанесения сначала высушивают, например, с помощью ИК-излучателя, а затем с применением УФ-излучателя при значениях длины волны от 120 до 350 нм, предпочтительно от 150 до 250 нм, особенно предпочтительно от 170 до 200 нм (например, 172 нм), отверждают под воздействием инертного газа. При этом предпочтительно отверждать не весь акрилатный слой, а только слой 0,1-0,5 нм. Это соответствует приблизительно 1 мг/м.The at least one acrylate-containing dispersion material is first dried after application, for example with an IR emitter and then with a UV emitter at wavelengths from 120 to 350 nm, preferably from 150 to 250 nm, particularly preferably from 170 to 200 nm (eg 172 nm), cured under the influence of an inert gas. In this case, it is preferable to cure not the entire acrylate layer, but only a layer of 0.1-0.5 nm. This corresponds to approximately 1 mg/m.

Возможными инертными газами являются азот, аргон, криптон, фтор, ксенон, KrCl, ArF, KRF, XeBr, XeCl, XeF, причем применение азота является особенно предпочтительным.Possible inert gases are nitrogen, argon, krypton, fluorine, xenon, KrCl, ArF, KRF, XeBr, XeCl, XeF, the use of nitrogen being particularly preferred.

В еще одном варианте осуществления способа согласно настоящему изобретению по меньшей мере один материал-основа имеет форму слоя бумаги, предпочтительно декоративного слоя бумаги или слоя бумаги-оверлей.In yet another embodiment of the method according to the present invention, at least one base material is in the form of a paper ply, preferably a decorative paper ply or an overlay paper ply.

Если в качестве материала-основы применяется слой бумаги, способ согласно настоящему изобретению включает следующие этапы:If a layer of paper is used as the base material, the method according to the present invention includes the following steps:

- нанесение по меньшей мере одного первого слоя из по меньшей мере одной порошкообразной смолы на по меньшей мере одну сторону слоя бумаги и плавление по меньшей мере одного нанесенного слоя из порошкообразной смолы;applying at least one first layer of at least one powdered resin to at least one side of the paper layer and melting at least one applied layer of powdered resin;

- нанесение по меньшей мере одного дисперсионного материала, содержащего акрилат, на подплавленный слой смолы и- applying at least one dispersion material containing acrylate to the melted resin layer and

- высушивание и отверждение слоистой структуры.- drying and curing of the layered structure.

Покрытый таким образом слой бумаги, например декоративный слой бумаги или слой бумаги-оверлей, имеет степень блеска менее 10, предпочтительно менее 8, особенно предпочтительно менее 5, и его можно прессовать с опорной плитой, например плитой на основе древесного материала, такой как MDF или HDF.The paper layer thus coated, such as a decorative paper layer or an overlay paper layer, has a gloss level of less than 10, preferably less than 8, particularly preferably less than 5, and can be pressed with a support board, for example a wood based board such as MDF or HDF.

В другом варианте осуществления в качестве материала-основы применяется плита на основе древесного материала, предпочтительно древесноволокнистая плита средней плотности (MDF), древесноволокнистая плита высокой плотности (HDF) или ориентированно-стружечная плита (OSB), клееная плита или плита на основе древесно-пластикового композита (WPC) или плита на основе каменно-пластикового композита (SPC).In another embodiment, the base material is a wood based board, preferably medium density fibreboard (MDF), high density fibreboard (HDF) or oriented strand board (OSB), glulam or wood plastic board. Composite (WPC) or Rock Plastic Composite (SPC) board.

В дополнительном варианте способ согласно настоящему изобретению включает следующие этапы:In an additional embodiment, the method according to the present invention includes the following steps:

- нанесение по меньшей мере одного первого слоя из по меньшей мере одной порошкообразной смолы на по меньшей мере одну сторону материала-основы, в частности плиты на основе древесного материала, и плавление по меньшей мере одного нанесенного слоя из порошкообразной смолы;- applying at least one first layer of at least one powdered resin to at least one side of the base material, in particular board based on wood material, and melting at least one applied layer of powdered resin;

- нанесение по меньшей мере одного декоративного слоя на по меньшей мере один подплавленный слой смолы посредством способа прямой печати;- applying at least one decorative layer to at least one melted resin layer by means of a direct printing method;

- нанесение по меньшей мере одного дополнительного второго слоя из по меньшей мере одной порошкообразной смолы на по меньшей мере один декоративный слой с нанесенной печатью;applying at least one additional second layer of at least one powdered resin to at least one decorative printed layer;

- плавление по меньшей мере одного слоя, нанесенного на декоративный слой, из порошкообразной смолы;- melting at least one layer deposited on the decorative layer of powdered resin;

- нанесение по меньшей мере одного дисперсионного материала, содержащего акрилат, на подплавленный слой смолы и- applying at least one dispersion material containing acrylate to the melted resin layer and

- высушивание и отверждение слоистой структуры.- drying and curing of the layered structure.

В одном варианте осуществления способа согласно настоящему изобретению порошкообразную смолу наносят в количестве от 10 до 100 г/м2, предпочтительно от 20 до 80 г/м2, в частности предпочтительно от 25 до 70 г/м2 на материал-основу. Это количество нанесения порошка смолы по существу относится ко всем слоям порошка смолы, которые должны быть нанесены, благодаря чему они могут быть адаптированы в каждом случае. Плотность распределения при этом выбирается таким образом, чтобы в каждом случае образовывались непрозрачные слои.In one embodiment of the process according to the present invention, the resin powder is applied in an amount of 10 to 100 g/m 2 , preferably 20 to 80 g/m 2 , particularly preferably 25 to 70 g/m 2 , to the base material. This resin powder application amount essentially refers to all layers of resin powder to be applied, whereby they can be adapted in each case. The distribution density is chosen in such a way that opaque layers are formed in each case.

Размер частиц порошкообразной смолы составляет от 20 до 100 мкм, предпочтительно от 40 до 80 мкм.The particle size of the powdered resin is 20 to 100 µm, preferably 40 to 80 µm.

В еще одном варианте осуществления способа согласно настоящему изобретению наносимая порошкообразная смола представляет собой формальдегидную смолу, предпочтительно карбамидную смолу или меламиновую смолу, особенно предпочтительно меламиноформальдегидную смолу. Предпочтительно применять меламиновую смолу или карбамидную смолу для первого слоя смолы. В верхних слоях предпочтительно используется только меламиновая смола.In yet another embodiment of the method according to the present invention, the applied resin powder is a formaldehyde resin, preferably a urea resin or a melamine resin, particularly preferably a melamine-formaldehyde resin. It is preferable to use melamine resin or urea resin for the first resin layer. Preferably only melamine resin is used in the top layers.

«Плавление» или «загустение» в контексте настоящей заявки означает, что слой смолы еще не полностью полимеризован, а скорее полимеризация останавливается на промежуточной стадии, на которой дальнейшее сшивание или полимеризация все еще возможны в более поздний момент обработки. Поэтому смысл «загустения» обычно основан на том факте, что в более поздний момент времени на уже нанесенный защитный слой должны быть нанесены дополнительные функциональные слои, иначе продукт будет готов только на дальнейших этапах обработки."Melting" or "thickening" in the context of this application means that the resin layer is not yet completely polymerized, but rather polymerization is stopped at an intermediate stage, at which further crosslinking or polymerization is still possible at a later point in processing. Therefore, the meaning of "thickening" is usually based on the fact that at a later point in time, additional functional layers must be applied to the already applied protective layer, otherwise the product will be ready only in further processing steps.

К порошку меламиновой смолы также могут быть добавлены другие вещества. Особенно предпочтительно при этом, что также из-за, например, эффектов, которые влияют на высаливание, загустение, осаждение и т.д., могут применяться вещества, которые плохо совместимы с жидкой меламиновой смолой. При этом это могут быть соли для увеличения электропроводимости, органические или неорганические огнезащитные средства, производные целлюлозы, поглотители радикалов, пигменты, поглотители УФ-излучения и т.д.Other substances may also be added to the melamine resin powder. It is particularly advantageous here that also because of, for example, effects that affect salting out, thickening, settling, etc., substances can be used that are poorly compatible with the liquid melamine resin. In this case, these can be salts to increase electrical conductivity, organic or inorganic flame retardants, cellulose derivatives, radical scavengers, pigments, UV radiation absorbers, etc.

Соответственно применяемая порошкообразная смола может содержать добавочные вещества, такие как пигменты, электропроводящие вещества и целлюлозу.Accordingly, the resin powder used may contain additive substances such as pigments, electrically conductive substances and cellulose.

При добавлении цветных пигментов слой подплавленного порошка смолы может одновременно служить белым грунтовочным слоем для декоративного слоя, на который впоследствии будет нанесена печать. В качестве цветных пигментов можно использовать белые пигменты, такие как диоксид титана (TiO2). Другими цветными пигментами могут быть карбонат кальция, сульфат бария или карбонат бария. Доля цветных пигментов может составлять до 50 вес.% от общего количества порошка.When colored pigments are added, the melted resin powder layer can simultaneously serve as a white primer layer for a decorative layer that will subsequently be printed. White pigments such as titanium dioxide (TiO 2 ) can be used as color pigments. Other color pigments may be calcium carbonate, barium sulfate or barium carbonate. The proportion of colored pigments can be up to 50% by weight of the total powder.

Добавление цветных пигментов к первому слою порошка смолы увеличивает укрывистость, так что его можно использовать в качестве (единственной) основы или грунтового покрытия для последующего декоративного слоя.The addition of colored pigments to the first layer of resin powder increases hiding power so that it can be used as a (sole) base or ground coat for a subsequent decorative layer.

Количество целлюлозных волокон, которые наносят с порошком смолы, может составлять от 0,1 до 1 вес.%, предпочтительно от 0,5 до 0,8 вес.% (в пересчете на наносимое количество смолы) или в диапазоне 0,1-0,5 г/м2, предпочтительно 0,2-0,4 г/м2, особенно предпочтительно 0,25 г/м2. Предпочтительно применяемые целлюлозные волокна бесцветны и имеют форму тонкого или гранулированного слегка гигроскопичного порошка.The amount of cellulosic fibers that are applied with the resin powder may be from 0.1 to 1 wt.%, preferably from 0.5 to 0.8 wt.% (based on the applied amount of resin) or in the range of 0.1-0 .5 g/m 2 , preferably 0.2-0.4 g/m 2 , particularly preferably 0.25 g/m 2 . Preferably, the cellulose fibers used are colorless and are in the form of a fine or granular, slightly hygroscopic powder.

Электропроводящие вещества могут быть выбраны из группы, включающей технический углерод, углеродные волокна, металлический порошок и наночастицы, в частности углеродные нанотрубки. Также можно применять комбинации этих веществ.The electrically conductive materials may be selected from the group consisting of carbon black, carbon fibers, metal powder and nanoparticles, in particular carbon nanotubes. Combinations of these substances can also be used.

Применяемые смолы содержат предпочтительно в каждом случае добавки, такие как отвердители, смачивающие средства (поверхностно-активные вещества или их смеси), антиадгезивы и/или другие компоненты.The resins used contain preferably in each case additives such as curing agents, wetting agents (surfactants or mixtures thereof), release agents and/or other components.

В предпочтительном варианте осуществления порошок смолы наносят посредством электростатического заряда. Нанесение также может быть выполнено посредством нанесения порошка после способа на основе трибостатического эффекта. В данном случае происходит заряд наносимого порошка в результате трения.In a preferred embodiment, the resin powder is applied by means of an electrostatic charge. The application can also be carried out by applying the powder after the tribostatic method. In this case, the applied powder is charged as a result of friction.

Плавление нанесенного слоя из порошкообразной смолы может происходить с применением ИК-излучателя, или также микроволновых систем или т. п. Особенно предпочтительно применение ИК-излучателей.The melting of the deposited resin powder layer can take place using an IR emitter, or also microwave systems or the like. The use of IR emitters is particularly preferred.

В одном варианте осуществления поверхность материала-основы, в частности в случае плиты на основе древесного материала, может быть предварительно обработана перед нанесением печати для улучшения адгезии последующих слоев. Это может быть чистка щетками, шлифовка, при которой также удаляются неровности с поверхности, и/или обработка плазмой или коронным разрядом.In one embodiment, the surface of the base material, in particular in the case of wood-based board, may be pre-treated prior to printing to improve the adhesion of subsequent layers. This may be brushing, grinding, which also removes surface irregularities, and/or plasma or corona treatment.

В предпочтительном варианте осуществления на следующем этапе на (первый) подплавленный слой порошка смолы наносят по меньшей мере одно грунтовое покрытие для повышения укрывистости краски.In a preferred embodiment, in the next step, at least one primer coat is applied to the (first) melted layer of resin powder to increase the covering power of the paint.

Грунтовое покрытие предпочтительно содержит казеин, кукурузный крахмал или соевый белок и может содержать неорганические цветовые пигменты и, таким образом, служить слоем грунтового покрытия для декоративного слоя, на котором впоследствии будет нанесена печать.The ground coat preferably contains casein, corn starch or soy protein and may contain inorganic color pigments and thus serve as a ground coat layer for a decorative layer which will subsequently be printed.

Белые пигменты, такие как диоксид титана (TiO2), в свою очередь, могут применяться в качестве цветных пигментов. Дополнительными цветными пигментами могут быть карбонат кальция, сульфат бария или карбонат бария, а также пигменты оксида железа (для коричневатого грунтового покрытия). Помимо цветных пигментов и казеина, кукурузного крахмала или соевого белка, грунтовое покрытие также может содержать воду в качестве растворителя.White pigments such as titanium dioxide (TiO 2 ) can in turn be used as color pigments. Additional color pigments can be calcium carbonate, barium sulfate or barium carbonate, as well as iron oxide pigments (for a brownish primer). In addition to color pigments and casein, corn starch or soy protein, the primer may also contain water as a solvent.

Количество наносимого жидкого грунтового покрытия может составлять от 10 до 50 г/м2, предпочтительно от 15 до 30 г/м2, особенно предпочтительно от 20 до 25 г/м2.The amount of liquid primer applied can be from 10 to 50 g/m 2 , preferably from 15 to 30 g/m 2 , particularly preferably from 20 to 25 g/m 2 .

Также возможно, что грунтовое покрытие состоит из по меньшей мере одного, предпочтительно из по меньшей мере двух или более нанесенных друг за другом слоев или покрытий (например, до пяти покрытий), при этом количество нанесения между слоями или покрытиями одинаковое или разное, то есть количество нанесения для каждого отдельного слоя может варьироваться.It is also possible that the ground coat consists of at least one, preferably of at least two or more layers or coatings applied one after the other (for example, up to five coatings), while the number of applications between layers or coatings is the same or different, i.e. the amount of application for each individual layer may vary.

Грунтовое покрытие можно нанести с применением валика на материал-основу, например плиту на основе древесного материала, с последующим высушиванием. Также возможно нанесение грунтового покрытия на материал-основу с помощью цифровой печати. Жидкие краски для цифровой печати, применяемые для цифровой печати грунтового покрытия, предпочтительно основаны на жидких УФ-красках, обогащенных пигментами белого цвета. Однако также можно применять жидкие краски для цифровой печати на водной основе или так называемые гибридные жидкие краски. Нанесение с использованием цифровой печати является предпочтительным, потому что система печати значительно короче, чем устройство в виде валика, и, таким образом, экономятся место, энергия и затраты.The primer coat can be applied using a roller to a base material, such as wood-based board, followed by drying. It is also possible to apply a ground coat to the base material using digital printing. Digital ink liquid inks used for groundcoat digital printing are preferably based on liquid UV inks enriched with white pigments. However, it is also possible to use water-based liquid inks for digital printing or so-called hybrid liquid inks. Application using digital printing is preferred because the printing system is much shorter than a roller device and thus saves space, energy and costs.

В еще одном варианте способа согласно настоящему изобретению на грунтовое покрытие наносят грунтовочный слой, предпочтительно в виде однократного нанесения с последующим высушиванием. Грунтовочный слой особенно полезен в случае последующего способа глубокой печати (с использованием валиков), в то время как при способе процесса цифровой печати он не является обязательно необходимым.In yet another embodiment of the method according to the present invention, a primer coat is applied to the primer coat, preferably as a single application followed by drying. The primer layer is particularly useful in the case of the subsequent gravure printing process (using rollers), while it is not necessarily necessary in the digital printing process process.

Количество нанесенной жидкой грунтовки составляет от 10 до 30 г/м2, предпочтительно от 15 до 20 г/м2. В качестве грунтовки предпочтительно применять соединения на основе полиуретана.The amount of liquid primer applied is 10 to 30 g/m 2 , preferably 15 to 20 g/m 2 . As a primer, it is preferable to use compounds based on polyurethane.

Способы глубокой печати и цифровой печати предпочтительно используются в качестве способов прямой печати для нанесения печати на плиты на основе древесного материала. Способ глубокой печати представляет собой технологию печати, в которой элементы, которые должны быть отображены, присутствуют в виде углублений в печатной форме и окрашены перед печатью. Печатная краска находится в основном в углублениях и переносится на печатаемый объект, такой как, например, материал-основа, в результате давления прижима печатной формы и сил сцепления. При применении непрямой глубокой печати используются несколько прижимных валиков.Gravure printing and digital printing methods are preferably used as direct printing methods for printing wood-based boards. The gravure printing method is a printing technology in which elements to be displayed are present as recesses in a printing plate and colored before printing. The printing ink resides mainly in the depressions and is transferred to the printed object, such as, for example, the base material, as a result of the pressing pressure of the printing plate and adhesive forces. When using indirect gravure printing, multiple pressure rollers are used.

В особенно предпочтительном варианте осуществления по меньшей мере один узор наносят на материал-основу (с обработанной поверхностью и предварительно нанесенным покрытием) с помощью способа цифровой печати. При цифровой печати печатное изображение передается непосредственно с компьютера на печатную машину, такую как, например, лазерный принтер или струйный принтер. При этом применение статичной печатной формы не обязательно. Печать узора происходит по принципу струйной печати за один проход, при котором покрывается вся ширина верхней печатаемой стороны, при этом плиты перемещаются под печатающее устройство. Однако также возможно, чтобы опорная плита, на которую наносится печать, была остановлена под печатающим устройством, и чтобы оно проходило поверх поверхности по меньшей мере один раз во время печати.In a particularly preferred embodiment, at least one pattern is applied to the base material (surfaced and pre-coated) using a digital printing process. With digital printing, the printed image is transferred directly from a computer to a printing machine such as a laser printer or an inkjet printer. In this case, the use of a static printing form is not necessary. The pattern is printed according to the principle of inkjet printing in one pass, in which the entire width of the upper printed side is covered, while the plates are moved under the printing device. However, it is also possible for the base plate to be printed to be stopped under the printer and for it to pass over the surface at least once during printing.

Печатные краски объединены в отдельных рядах печатающих головок, при этом для каждого цвета может быть предусмотрен один или два ряда печатающих головок. Цветами жидких красок для цифровой печати являются, например, черный, синий, красный, рыжевато-желтый, зеленовато-желтый, необязательно также может применяться цветовая модель CMYK. Жидкие краски для цифровой печати необязательно основаны на тех же пигментах, которые применяются для аналоговой и/или цифровой печати с жидкими красками на водной основе. Жидкие краски для цифровой печати предпочтительно основаны на жидких УФ-красках. Однако также можно применять жидкие краски для цифровой печати на водной основе или так называемые гибридные жидкие краски. После печати декоративный отпечаток высушивают и/или облучают.Printing inks are combined in separate rows of printheads, and each color may have one or two rows of printheads. Liquid ink colors for digital printing are, for example, black, blue, red, tan, greenish yellow, optionally the CMYK color model can also be used. Liquid inks for digital printing are not necessarily based on the same pigments used for analog and/or digital printing with water-based liquid inks. Liquid inks for digital printing are preferably based on liquid UV inks. However, it is also possible to use water-based liquid inks for digital printing or so-called hybrid liquid inks. After printing, the decorative print is dried and/or irradiated.

Печатные краски наносятся в количестве от 1 до 30 г/м2, предпочтительно от 3 до 20 г/м2, особенно предпочтительно от 3 до 15 г/м2.Printing inks are applied in an amount of 1 to 30 g/m 2 , preferably 3 to 20 g/m 2 , particularly preferably 3 to 15 g/m 2 .

Вместе с узором наносят также метки, необходимые для ориентации в прессе.Along with the pattern, the marks necessary for orientation in the press are also applied.

Дополнительный слой порошкообразной смолы, нанесенный и подплавленный на декоративном слое, предпочтительно содержит порошок на основе формальдегидной смолы, особенно предпочтительно меламиноформальдегидной смолы. Количество нанесения порошка смолы на этом этапе составляет от 10 до 50 г/м2, предпочтительно от 20 до 40 г/м2.The additional layer of powdered resin deposited and melted on the decorative layer preferably contains a powder based on formaldehyde resin, particularly preferably melamine-formaldehyde resin. The application amount of the resin powder in this step is 10 to 50 g/m 2 , preferably 20 to 40 g/m 2 .

Как уже указывалось выше, добавочные вещества, такие как электропроводящие вещества или целлюлоза, и добавки, такие как отвердители, смачивающие средства или антиадгезивы, также могут быть добавлены в порошок смолы на этом этапе способа.As mentioned above, additives such as electrically conductive substances or cellulose and additives such as hardeners, wetting agents or release agents can also be added to the resin powder at this stage of the process.

Плавление или загустение в данном случае также происходит предпочтительно с применением ИК-излучателя.Melting or thickening in this case also takes place preferably using an IR emitter.

После этого этапа способа можно отправить материал-основу с нанесенной печатью на промежуточное хранение. Нанесенный и подплавленный слой порошка смолы служит в этом случае защитным слоем, который, с одной стороны, служит для защиты поверхности с нанесенной печатью в случае промежуточного хранения, а с другой стороны (из-за еще не полностью затвердевшего слоя смолы) обеспечивает возможность дополнительной обработки. В частности, в случае сложных процессов обработки необходимо разделение определенных этапов работы по причинам стоимости, технологии и т.д. Например, связанные производственные линии могут сильно различаться в отношении своей производительности. Затем нужно сформировать буферный склад, в котором материалы укладывают друг на друга. Кроме того, на производственной линии может потребоваться несколько циклов, поскольку количество нанесения и т.п. не могут быть реализованы за один цикл. Во всех этих случаях предпочтительны высушенные или затвердевшие поверхности, поскольку они, с одной стороны, обеспечивают защиту поверхности с нанесенной печатью в случае промежуточного хранения и, с другой стороны, дополнительную обработку.After this process step, the printed base material can be sent to intermediate storage. The applied and melted layer of resin powder serves in this case as a protective layer, which, on the one hand, serves to protect the printed surface in the event of intermediate storage, and on the other hand (due to the not yet completely hardened resin layer) allows additional processing. . Particularly in the case of complex machining processes, it is necessary to separate certain work steps for reasons of cost, technology, etc. For example, related product lines can vary greatly in terms of their performance. Then you need to form a buffer warehouse in which the materials are stacked on top of each other. In addition, several cycles may be required on the production line, since the amount of application, etc. cannot be realized in one cycle. In all these cases, dried or hardened surfaces are preferred, since on the one hand they provide protection for the printed surface in case of intermediate storage and, on the other hand, additional processing.

В дополнительном варианте осуществления износостойкие частицы равномерно распределяют на декоративном слое или на слое порошка смолы, нанесенном на декоративный слой.In a further embodiment, the wear resistant particles are uniformly distributed on the decorative layer or on the resin powder layer deposited on the decorative layer.

В качестве износостойких частиц могут применяться корунд (оксид алюминия), карбид бора, диоксид кремния, частицы карбида кремния. Особенно предпочтительными являются частицы из корунда. При этом речь идет предпочтительно об электрокорунде (белом) высшего качества с высокой степенью прозрачности, так что негативное воздействие на визуальный эффект нижележащего узора является максимально малым. Корунд имеет неравномерную пространственную форму.Corundum (aluminum oxide), boron carbide, silicon dioxide, silicon carbide particles can be used as wear-resistant particles. Corundum particles are especially preferred. In this case, it is preferably high quality electrocorundum (white) with a high degree of transparency, so that the visual effect of the underlying pattern is adversely affected as little as possible. Corundum has an uneven spatial shape.

Количество распределенных износостойких частиц составляет от 7 до 50 г/м2, предпочтительно от 10 до 30 г/м2, особенно предпочтительно от 15 до 25 г/м2. Количество распределенных износостойких частиц зависит от класса износа, который должен быть достигнут, и размера зерен. Таким образом, количество износостойких частиц в случае класса износа AC3 находится в диапазоне от 10 до 15 г/м2, в случае класса износа AC4 от 15 до 20 г/м2 и в случае класса износа AC5 от 20 до 35 г/м2 при применении зернистости F200. В настоящем случае готовые плиты обладают предпочтительно классом износа AC4.The amount of wear particles distributed is 7 to 50 g/m 2 , preferably 10 to 30 g/m 2 , particularly preferably 15 to 25 g/m 2 . The amount of wear particles distributed depends on the wear class to be achieved and the grain size. Thus, the amount of wear-resistant particles in the case of wear class AC3 is in the range from 10 to 15 g/m 2 , in the case of wear class AC4 from 15 to 20 g/m 2 and in the case of wear class AC5 from 20 to 35 g/m 2 when using grit size F200. In the present case, the finished boards preferably have wear class AC4.

Применяют износостойкие частицы с зернистостью классов F180-F240, предпочтительно F200. Размер зерен класса F180 находится в диапазоне 53-90 мкм, F220 - 45-75 мкм, F230 - 34-82 мкм, F240 - 28-70 мкм (согласно стандарту FEPA). В одном варианте в качестве износостойких частиц применяется белый электрокорунд высшего качества F180-F240, предпочтительно с основным диапазоном размера зерен 53-90 мкм. В особенно предпочтительном варианте осуществления применяют частицы из корунда класса F180-220.Use wear-resistant particles with grit classes F180-F240, preferably F200. The grain size of class F180 is in the range of 53-90 µm, F220 - 45-75 µm, F230 - 34-82 µm, F240 - 28-70 µm (according to the FEPA standard). In one embodiment, premium white fused aluminum oxide F180-F240 is used as wear resistant particles, preferably with a main grain size range of 53-90 μm. In a particularly preferred embodiment, corundum grade F180-220 particles are used.

Износостойкие частицы не должны быть слишком мелкозернистыми (опасность образования пыли), но также не должны быть слишком крупнозернистыми. Поэтому размер износостойких частиц является адаптивным.The wear-resistant particles must not be too fine (danger of dust formation) but also not too coarse. Therefore, the size of wear-resistant particles is adaptive.

В приведенном далее варианте осуществления можно применять силанизированные частицы из корунда. Типичными силанизирующими средствами являются аминосиланы.In the following embodiment, silanized corundum particles can be used. Typical silanizing agents are aminosilanes.

В дополнительном варианте осуществления способа согласно настоящему изобретению по меньшей мере один третий слой из по меньшей мере одной порошкообразной смолы наносят, в частности, на слой из износостойких частиц. Этот слой служит в качестве разделительного слоя для ограждения износостойких частиц.In a further embodiment of the method according to the present invention, at least one third layer of at least one powdered resin is applied, in particular on the layer of wear-resistant particles. This layer serves as a separating layer to enclose wear resistant particles.

Слой порошкообразной смолы, нанесенный и подплавленный на этом этапе, в частности на износостойких частицах, содержит предпочтительно порошок на основе формальдегидной смолы, особенно предпочтительно меламиноформальдегидной смолы. Количество нанесения порошка смолы на этом этапе составляет от 10 до 50 г/м2, предпочтительно от 20 до 40 г/м2.The layer of powdered resin deposited and melted in this step, in particular on the wear-resistant particles, preferably contains a powder based on formaldehyde resin, particularly preferably melamine-formaldehyde resin. The application amount of the resin powder in this step is 10 to 50 g/m 2 , preferably 20 to 40 g/m 2 .

Как уже указывалось выше, добавочные вещества, такие как электропроводящие вещества или целлюлоза, и добавки, такие как отвердители, смачивающие средства или антиадгезивы, также могут быть добавлены в порошок смолы на этом этапе способа.As mentioned above, additives such as electrically conductive substances or cellulose and additives such as hardeners, wetting agents or release agents can also be added to the resin powder at this stage of the process.

Плавление или загустение в данном случае также происходит предпочтительно с применением ИК-излучателя.Melting or thickening in this case also takes place preferably using an IR emitter.

В дополнительном варианте осуществления способа согласно настоящему изобретению стеклянные шарики распределяют, в частности, на по меньшей мере одном третьем подплавленном слое порошка смолы. Стеклянные шарики служат в качестве разделителя между износостойкими частицами и последующей пластиной для прессования. Таким образом можно по крайней мере частично снизить истирание пластины.In a further embodiment of the method according to the present invention, the glass beads are distributed, in particular, on at least one third subfused resin powder layer. The glass beads serve as a separator between the wear particles and the subsequent pressing plate. In this way, wear of the insert can be at least partially reduced.

Предпочтительно применяемые стеклянные шарики имеют диаметр 60-120 мкм, предпочтительно 80-90 мкм. Диаметр стеклянных шариков соответствует среднему размеру применяемых износостойких частиц, чтобы обеспечить оптимальное ограждение для последующей пластины для прессования. Следовательно, в случае корунда F220 применяются стеклянные шарики с диаметром 70-90 мкм, а в случае корунда F180 применяются стеклянные шарики с диаметром 80-120 мкм.Preferably the glass beads used have a diameter of 60-120 µm, preferably 80-90 µm. The diameter of the glass beads corresponds to the average size of the applied wear particles in order to provide optimal enclosing for the subsequent pressing plate. Therefore, in the case of corundum F220, glass beads with a diameter of 70-90 µm are used, and in the case of corundum F180, glass beads with a diameter of 80-120 µm are used.

Количество стеклянных шариков составляет от 5 до 30 г/м2, предпочтительно от 8 до 20 г/м2, особенно предпочтительно от 8 до 15 г/м2.The amount of glass beads is 5 to 30 g/m 2 , preferably 8 to 20 g/m 2 , particularly preferably 8 to 15 g/m 2 .

Стеклянные шарики также могут присутствовать в силанизированной форме. Благодаря силанизированию стеклянных шариков улучшается запрессовывание стеклянных бусинок в матрицу смолы.The glass beads may also be present in silanized form. By silanizing the glass beads, the pressing of the glass beads into the resin matrix is improved.

В дополнительном варианте осуществления способа согласно настоящему изобретению по меньшей мере один дополнительный, например, четвертый слой из по меньшей мере одной порошкообразной смолы наносят, в частности, на слой из стеклянных шариков. Этот слой служит для ограждения стеклянных шариков и в качестве отделочного слоя.In a further embodiment of the method according to the present invention, at least one additional, for example, a fourth layer of at least one powdered resin is applied, in particular, to a layer of glass beads. This layer serves to enclose the glass beads and as a finishing layer.

Дополнительный четвертый слой порошкообразной смолы, нанесенный и подплавленный на этом этапе, в частности на стеклянных шариках, содержит предпочтительно порошок на основе формальдегидной смолы, особенно предпочтительно меламиноформальдегидной смолы. Количество нанесения порошка смолы на этом этапе составляет от 10 до 50 г/м2, предпочтительно от 20 до 40 г/м2.The additional fourth layer of powdered resin deposited and melted in this step, in particular on glass beads, preferably contains powder based on formaldehyde resin, particularly preferably melamine-formaldehyde resin. The application amount of the resin powder in this step is 10 to 50 g/m 2 , preferably 20 to 40 g/m 2 .

Как уже указывалось выше, добавочные вещества, такие как электропроводящие вещества или целлюлоза, и добавки, такие как отвердители, смачивающие средства или антиадгезивы, также могут быть добавлены в порошок смолы на этом этапе способа.As mentioned above, additives such as electrically conductive substances or cellulose and additives such as hardeners, wetting agents or release agents can also be added to the resin powder at this stage of the process.

Плавление или загустение в данном случае также происходит предпочтительно с применением ИК-излучателя.Melting or thickening in this case also takes place preferably using an IR emitter.

В еще одном варианте осуществления способа согласно настоящему изобретению прессуют слоистую структуру в прессе с коротким циклом (KT-прессе). Этап прессования происходит под воздействием давления и температуры от 180 до 250°C, предпочтительно от 200 до 230°C, особенно предпочтительно при температуре 200°C и давлении от 30 до 60 кг/см2, особенно предпочтительно от 40 до 50 кг/см2. Время прессования составляет от 8 до 30 c, предпочтительно от 10 до 25 c.In yet another embodiment of the method according to the present invention, the laminar structure is pressed in a short cycle press (KT press). The pressing step takes place under pressure and a temperature of 180 to 250°C, preferably 200 to 230°C, particularly preferably at a temperature of 200°C and a pressure of 30 to 60 kg/cm 2 , particularly preferably 40 to 50 kg/cm 2 . The pressing time is 8 to 30 seconds, preferably 10 to 25 seconds.

Предпочтительно покрытый материал-основа, такой как покрытая плита на основе древесного материала в прессе с коротким циклом ориентирована относительно структурированной пластины для прессования, находящейся в прессе с коротким циклом, в зависимости от меток на плите на основе древесного материала, таким образом получают совпадение узора на плите на основе древесного материала и вытисненной структуры пластины для прессования. Это обеспечивает получение структуры, совпадающей с узором. В ходе прессования происходит плавление слоев меламиновой смолы и формирование слоистого материала во время реакции конденсации с включением таких компонентов, как корунд/стекло/волокна.Preferably, the coated base material, such as the coated wood based board in the short cycle press, is oriented relative to the structured press plate in the short cycle press, depending on the marks on the wood based board, thus obtaining pattern matching on a board based on wood material and an embossed structure of a pressing plate. This provides a structure that matches the pattern. During pressing, the layers of melamine resin are melted and the laminate is formed during the condensation reaction with the inclusion of components such as corundum/glass/fibers.

На нижней стороне плиты на основе древесного материала может быть нанесен стабилизирующий слой, например, из нескольких слоев смолы, без добавочных веществ или бумажного стабилизирующего слоя. Это гарантирует, что растягивающие силы на плите на основе древесного материала, создаваемые нанесенными слоями при прессовании, компенсируют друг друга. Стабилизирующий слой, нанесенный на нижнюю сторону, соответствует слоистой структуре, и соответствующая толщина слоя приблизительно соответствует последовательности слоев, нанесенных на верхнюю сторону, но без добавления добавочных веществ, износостойких частиц или стеклянных шариков. Также пропитанный слой можно применять в качестве стабилизирующего слоя.On the underside of the wood-based board, a stabilizing layer can be applied, for example, from several layers of resin, without additives or a paper stabilizing layer. This ensures that the tensile forces on the wood-based board created by the applied layers during pressing cancel each other out. The stabilizing layer applied to the bottom side corresponds to the layered structure and the corresponding layer thickness approximately corresponds to the sequence of layers applied to the top side, but without the addition of additives, wear particles or glass beads. The impregnated layer can also be used as a stabilizing layer.

В предпочтительном первом варианте осуществления способ согласно настоящему изобретению включает следующие этапы:In a preferred first embodiment, the method according to the present invention includes the following steps:

- нанесение по меньшей мере одного первого слоя из по меньшей мере одной порошкообразной смолы на по меньшей мере одну сторону плиты на основе древесного материала и плавление по меньшей мере одного нанесенного слоя из порошкообразной смолы;applying at least one first layer of at least one powdered resin to at least one side of the wood-based board and melting the at least one applied layer of powdered resin;

- нанесение по меньшей мере одного грунтового покрытия на первый подплавленный слой порошка смолы;- applying at least one primer coating on the first sub-melted layer of resin powder;

- нанесение по меньшей мере одного грунтовочного слоя на по меньшей мере одно грунтовое покрытие;- applying at least one primer layer to at least one primer coat;

- нанесение по меньшей мере одного декоративного слоя посредством способа прямой печати;- applying at least one decorative layer by means of a direct printing method;

- распределение износостойких частиц;- distribution of wear-resistant particles;

- нанесение по меньшей мере одного дополнительного слоя из по меньшей мере одной порошкообразной смолы на по меньшей мере один слой из износостойких частиц и плавление нанесенного слоя из порошкообразной смолы;- applying at least one additional layer of at least one powdered resin on at least one layer of wear-resistant particles and melting the applied layer of powdered resin;

- нанесение, высушивание и отверждение по меньшей мере одного дисперсионного материала, содержащего акрилат, на подплавленном слое смолы и- applying, drying and curing at least one dispersion material containing acrylate on the melted resin layer and

- прессование слоистой структуры.- pressing a layered structure.

В предпочтительном дополнительном варианте осуществления способ согласно настоящему изобретению включает следующие этапы:In a preferred further embodiment, the method according to the present invention includes the following steps:

- нанесение по меньшей мере одного первого слоя из по меньшей мере одной порошкообразной смолы на по меньшей мере одну сторону плиты на основе древесного материала и плавление по меньшей мере одного нанесенного слоя из порошкообразной смолы;applying at least one first layer of at least one powdered resin to at least one side of the wood-based board and melting the at least one applied layer of powdered resin;

- нанесение по меньшей мере одного грунтового покрытия на первый подплавленный слой порошка смолы;- applying at least one primer coating on the first sub-melted layer of resin powder;

- нанесение по меньшей мере одного грунтовочного слоя на по меньшей мере одно грунтовое покрытие;- applying at least one primer layer to at least one primer coat;

- нанесение по меньшей мере одного декоративного слоя посредством способа прямой печати;- applying at least one decorative layer by means of a direct printing method;

- нанесение по меньшей мере одного второго слоя из по меньшей мере одной порошкообразной смолы на по меньшей мере один декоративный слой с нанесенной печатью и плавление по меньшей мере одного второго слоя из порошкообразной смолы, нанесенного на декоративный слой;applying at least one second layer of at least one resin powder to at least one printed decorative layer and melting at least one second layer of resin powder applied to the decorative layer;

- распределение износостойких частиц;- distribution of wear-resistant particles;

- нанесение по меньшей мере одного дополнительного третьего слоя из по меньшей мере одной порошкообразной смолы на по меньшей мере один слой из износостойких частиц и плавление нанесенного третьего слоя из порошкообразной смолы;- applying at least one additional third layer of at least one powdered resin on at least one layer of wear-resistant particles and melting the applied third layer of powdered resin;

- распределение стеклянных шариков на по меньшей мере одном третьем подплавленном слое порошка смолы;- the distribution of glass beads on at least one third subfused layer of resin powder;

- нанесение по меньшей мере одного дополнительного четвертого слоя из по меньшей мере одной порошкообразной смолы на слой из стеклянных шариков и плавление нанесенного четвертого слоя из порошкообразной смолы;- applying at least one additional fourth layer of at least one powdered resin to the layer of glass beads and melting the applied fourth layer of powdered resin;

- нанесение, высушивание и отверждение по меньшей мере одного дисперсионного материала, содержащего акрилат, на подплавленном слое смолы и- applying, drying and curing at least one dispersion material containing acrylate on the melted resin layer and

- прессование слоистой структуры.- pressing a layered structure.

Таким образом, способ согласно настоящему изобретению обеспечивает возможность получения стойкой к истиранию, снабженной декоративным слоем и матированной плиты на основе древесного материала со структурой смолы с износостойкими частицами. Плита на основе древесного материала согласно настоящему изобретению имеет степень блеска менее 10, предпочтительно менее 8, особенно предпочтительно менее 5, например, от 3,4 или 3,8 единицы блеска.Thus, the method according to the present invention makes it possible to obtain an abrasion-resistant, decorative-layered and frosted wood-based board with a resin structure with wear-resistant particles. The wood based board according to the invention has a gloss level of less than 10, preferably less than 8, particularly preferably less than 5, for example from 3.4 or 3.8 gloss units.

Плита на основе древесного материала содержит по меньшей мере один декоративный слой на верхней стороне и многослойную структуру смолы, содержащую износостойкие частицы, необязательно целлюлозные волокна и стеклянные шарики, при этом многослойная структура смолы имеет толщину всего слоя от 60 до 200 мкм, предпочтительно от 90 до 150 мкм, особенно предпочтительно от 100 до 120 мкм.The wood-based board comprises at least one decorative layer on the top side and a resin multilayer structure containing wear-resistant particles, optionally cellulose fibers and glass beads, the resin multilayer structure having an entire layer thickness of 60 to 200 µm, preferably 90 to 150 µm, particularly preferably 100 to 120 µm.

В одном варианте осуществления способ согласно настоящему изобретению обеспечивает возможность получения износостойкой плиты на основе древесного материала со следующей слоистой структурой (если смотреть снизу вверх): необязательно стабилизирующий слой - плита на основе древесного материала - первый слой смолы из подплавленного порошка смолы - декоративный слой с нанесенной печатью - второй слой смолы из подплавленного порошка смолы (защитный слой) - отвержденный акрилатный слой.In one embodiment, the method according to the present invention makes it possible to obtain a wood based wear board with the following layered structure (viewed from bottom to top): optionally a stabilizing layer - wood based board - first resin layer of melted resin powder - decorative layer with applied printing - the second resin layer of melted resin powder (protective layer) - cured acrylate layer.

В еще одном варианте осуществления способ согласно настоящему изобретению обеспечивает возможность получения износостойкой плиты на основе древесного материала со следующей слоистой структурой (если смотреть снизу вверх): необязательно стабилизирующий слой - плита на основе древесного материала - первый слой смолы из подплавленного порошка смолы - слой грунтового покрытия - грунтовочный слой - декоративный слой с нанесенной печатью - слой из износостойких частиц - второй слой смолы из подплавленного порошка смолы (защитный слой) - отвержденный акрилатный слой.In yet another embodiment, the method according to the present invention makes it possible to obtain a wear-resistant wood based board with the following layer structure (viewed from bottom to top): optional stabilizing layer - wood based board - first resin layer of melted resin powder - ground coating layer - a primer layer - a printed decorative layer - a layer of wear-resistant particles - a second resin layer of melted resin powder (protective layer) - a cured acrylate layer.

В еще одном варианте осуществления способ согласно настоящему изобретению обеспечивает возможность получения износостойкой плиты на основе древесного материала со следующей слоистой структурой (если смотреть снизу вверх): необязательный стабилизирующий слой - плита на основе древесного материала - первый слой смолы из подплавленного порошка смолы - слой грунтового покрытия - грунтовочный слой - декоративный слой с нанесенной печатью - второй слой смолы из подплавленного порошка смолы (защитный слой) - слой из износостойких частиц - третий слой смолы из подплавленного порошка смолы (разделительный слой) - стеклянные шарики (разделитель) - четвертый слой смолы из подплавленного порошка смолы - отвержденный акрилатный слой.In yet another embodiment, the method according to the present invention provides a possibility to obtain a wear resistant wood based board with the following layered structure (viewed from bottom to top): optional stabilizing layer - wood based board - first resin layer of melted resin powder - ground coat layer - primer layer - printed decorative layer - second resin layer of melted resin powder (protective layer) - layer of wear-resistant particles - third layer of resin of melted resin powder (separation layer) - glass beads (separator) - fourth resin layer of melted resin resin powder - cured acrylate layer.

Защитный слой служит для покрытия узора и защиты узора во время промежуточного хранения (укладка в слои, хранение, транспортировка). Дополнительные слои смолы на верхней стороне образуют в целом защитную пленку, которая защищает готовый слоистый материал от износа и обеспечивает структурирование, совпадающее с узором.The protective layer serves to cover the pattern and protect the pattern during intermediate storage (layering, storage, transportation). The additional layers of resin on the top side form an overall protective film that protects the finished laminate from wear and provides structuring that matches the pattern.

Производственная линия для выполнения способа согласно настоящему изобретению содержит следующие элементы:The production line for carrying out the method according to the present invention contains the following elements:

- по меньшей мере одно устройство для нанесения, предназначенное для нанесения слоя порошка смолы, который может содержать волокна, на верхнюю сторону материала-основы;- at least one application device for applying a layer of resin powder, which may contain fibers, on the upper side of the base material;

- по меньшей мере одно устройство для плавления первого слоя порошка смолы, в частности, ИК-излучатель;- at least one device for melting the first layer of resin powder, in particular an IR emitter;

- по меньшей мере одно устройство для нанесения, предназначенное для нанесения по меньшей мере одного дисперсионного материала, содержащего акрилат, на подплавленный слой смолы, иat least one applicator for applying at least one acrylate-containing dispersion material to the melted resin layer, and

- по меньшей мере одно устройство для отверждения акрилатсодержащего слоя, в частности, УФ-излучатель.- at least one device for curing the acrylate-containing layer, in particular a UV emitter.

В одном предпочтительном варианте осуществления производственная линия согласно настоящему изобретению содержит следующие элементы:In one preferred embodiment, the production line according to the present invention contains the following elements:

- по меньшей мере одно устройство для нанесения, предназначенное для нанесения первого слоя порошка смолы, который может содержать волокна, на верхнюю сторону плиты на основе древесного материала в качестве материала-основы и по меньшей мере одно устройство для плавления первого слоя порошка смолы, в частности, ИК-излучатель;- at least one application device for applying a first layer of resin powder, which may contain fibers, on the top side of the board based on wood material as a base material and at least one device for melting the first layer of resin powder, in particular , IR emitter;

- необязательно по меньшей мере одно устройство для нанесения, предназначенное для нанесения по меньшей мере одного слоя грунтового покрытия;optionally at least one applicator for applying at least one primer coat;

- необязательно по меньшей мере одно устройство для нанесения, предназначенное для нанесения по меньшей мере одного грунтовочного слоя;- optionally at least one application device for applying at least one primer layer;

- по меньшей мере одно устройство для нанесения печати;- at least one printing device;

- необязательно по меньшей мере одно устройство для нанесения, предназначенное для нанесения дополнительного слоя порошка смолы, и по меньшей мере одно устройство для плавления слоя порошка смолы, в частности, ИК-излучатель;- optionally at least one application device for applying an additional layer of resin powder, and at least one device for melting the layer of resin powder, in particular an IR emitter;

- необязательно по меньшей мере одно устройство для распределения предварительно определенного количества износостойких частиц;- optionally at least one device for distributing a predetermined amount of wear-resistant particles;

- необязательно по меньшей мере одно устройство для нанесения, предназначенное для нанесения дополнительного слоя порошка смолы, и по меньшей мере одно устройство для плавления слоя порошка смолы, в частности, ИК-излучатель;- optionally at least one application device for applying an additional layer of resin powder, and at least one device for melting the layer of resin powder, in particular an IR emitter;

- необязательно по меньшей мере одно устройство для распределения предварительно определенного количества стеклянных шариков;- optionally at least one device for dispensing a predetermined number of glass beads;

- необязательно по меньшей мере одно устройство для нанесения, предназначенное для нанесения дополнительного слоя порошка смолы, и по меньшей мере одно устройство для плавления первого слоя порошка смолы, в частности, ИК-излучатель;- optionally at least one application device for applying an additional layer of resin powder, and at least one device for melting the first layer of resin powder, in particular an IR emitter;

- по меньшей мере одно устройство для нанесения, предназначенное для нанесения по меньшей мере одного дисперсионного материала, содержащего акрилат, на подплавленный слой смолы, и по меньшей мере одно устройство для высушивания и отверждения акрилатсодержащего слоя, в частности, УФ-излучатель; иat least one applicator for applying at least one acrylate-containing dispersion material to the melted resin layer, and at least one applicator for drying and curing the acrylate-containing layer, in particular a UV emitter; And

- необязательно по меньшей мере один пресс с коротким циклом.optionally at least one short cycle press.

Трибостатические пистолеты могут применяться в качестве устройств, предусмотренных в производственной линии согласно настоящему изобретению, для нанесения слоев порошка смолы.Tribo guns can be used as devices provided in the production line according to the present invention for applying layers of resin powder.

Распределительное устройство для износостойких частиц и стеклянных шариков, предусмотренное в производственной линии согласно настоящему изобретению, подходит для рассеивания порошка, гранул, волокон и содержит систему колеблющихся щеток. Распределительное устройство состоит по существу из накопительного бункера, вращающегося структурированного валика и скребка. При этом количество наносимого износостойкого материала определяется скоростью вращения валика. Распределительное устройство предпочтительно содержит заершенный валик.The dispensing device for wear-resistant particles and glass beads provided in the production line according to the present invention is suitable for dispersing powder, granules, fibers, and contains an oscillating brush system. The distribution device essentially consists of a storage hopper, a rotating structured roller and a scraper. In this case, the amount of applied wear-resistant material is determined by the speed of rotation of the roller. The distributing device preferably comprises a barbed roller.

Кроме того, в одном варианте осуществления производственной линии согласно настоящему изобретению предусмотрено, что по меньшей мере одно распределительное устройство окружено по меньшей мере одной камерой, которая снабжена по меньшей мере одним средством для удаления пыли, возникающей в камере, или расположено в ней. Средство для удаления пыли может быть выполнено в виде всасывающего устройства или также в виде устройства для продувки воздухом. Продувка воздухом может обеспечиваться посредством сопел, которые установлены на входе и выходе плиты и нагнетают воздух в камеру. Кроме того, они могут препятствовать созданию в результате движения воздуха неоднородной завесы распределения из износостойкого материала.In addition, in one embodiment of the production line according to the present invention, it is provided that at least one distribution device is surrounded by at least one chamber, which is provided with at least one means for removing dust arising in the chamber, or located in it. The dust removal means can be in the form of a suction device or also in the form of an air blowing device. Air blowing can be provided by means of nozzles that are installed at the inlet and outlet of the plate and force air into the chamber. In addition, they can prevent the creation of an inhomogeneous distribution curtain of wear-resistant material as a result of air movement.

Удаление пыли от износостойкого материала из окружающей среды распределительного устройства является предпочтительным, поскольку в дополнение к очевидному воздействию на здоровье работников, работающих на производственной линии, мелкая пыль от износостойких частиц также осаждается на других частях установки производственной линии и приводит к увеличенному истиранию. Следовательно, расположение распределительного устройства в камере не только снижает загрязнение окружающей среды производственной линии пылью и воздействие на здоровье, но и предотвращает преждевременное истирание.Removal of wear resistant material dust from the switchgear environment is advantageous because, in addition to the obvious health impacts of workers on the production line, fine dust from wear resistant particles is also deposited on other parts of the production line plant and leads to increased attrition. Therefore, the location of the dispensing device in the chamber not only reduces dust pollution and health effects of the production line, but also prevents premature abrasion.

Распределительное устройство предпочтительно управляется посредством фоторелейной завесы, при этом фоторелейная завеса расположена по направлению обработки перед валиком (распределяющим валиком), предусмотренным под распределяющим устройством. Управление распределительным устройством с помощью фоторелейной завесы имеет смысл, так как между отдельными плитами на основе древесного материала имеются более или менее большие зазоры, что запускает процесс распределения, как только плита оказывается перед распределяющим валиком.The spreading device is preferably controlled by means of a light curtain, the light curtain being located in the processing direction in front of a roller (spreading roller) provided below the spreading device. Controlling the spreader with a light curtain makes sense, since there are more or less large gaps between the individual boards based on wood-based material, which starts the spreading process as soon as the board is in front of the spreading roller.

В одном варианте осуществления представленного распределительного устройства перед распределяющим валиком предусмотрен по меньшей мере один бункер для улавливания излишних износостойких частиц (то есть частиц, которые не распределяются на по меньшей мере одну плиту на основе древесного материала, а распределяются скорее перед входом плиты на основе древесного материала с помощью подающего устройства под распределяющим валиком до падающих износостойких частиц).In one embodiment of the present distribution device, at least one bin is provided before the spreading roller to catch excess wear-resistant particles (that is, particles that are not distributed on at least one wood based material board, but are distributed rather before the entry of the wood based material board). by means of a feeder under the spreading roller to the falling wear-resistant particles).

В еще одном варианте воронка соединена с по меньшей мере одним транспортирующим устройством и одним просеивающим устройством, при этом собранный в бункере лишний износостойкий материал транспортируется посредством транспортирующего устройства в просеивающее устройство. Ячейки в сите просеивающего устройства соответствуют наибольшему размеру используемых крупинок материала в виде обеспечивающих износостойкость частиц (то есть приблизительно 80-100 мкм). Частицы грязи и комковатый материал (такой как комкованная смола или комкованный износостойкий материал) отделяются от собранного износостойкого материала в просеивающем устройстве, и просеянный износостойкий материал может быть возвращен обратно в распределительное устройство (переработан).In yet another embodiment, the funnel is connected to at least one conveying device and one screening device, while the excess wear-resistant material collected in the hopper is transported by means of the conveying device to the screening device. The cells in the sieve of the screening device correspond to the largest size of the used grains of material in the form of wear-resistant particles (ie, approximately 80-100 microns). Dirt particles and lumpy material (such as lumpy resin or lumpy wear material) are separated from the collected wear material in the screening device, and the screened wear material can be returned back to the distributor (recycled).

Как уже объяснено выше, также предусмотрено целенаправленное добавление отвердителя в соответствующие блоки нанесения или устройства для нанесения для различных слоев смолы для жидкой смолы. В одном варианте осуществления производственная линия согласно настоящему изобретению оснащена с этой целью по меньшей мере одной дозирующей установкой, предназначенной для добавления отвердителя в каждое устройство для нанесения. Отвердитель перекачивают из по меньшей мере одной дозирующей установки в приемную емкость для смолы и смешивают в приемной емкости со смолой, например посредством подходящей мешалки.As already explained above, it is also envisaged to selectively add the curing agent to the respective applicators or applicators for the different resin layers for the liquid resin. In one embodiment, the production line according to the present invention is equipped for this purpose with at least one dosing unit for adding hardener to each applicator. The hardener is pumped from the at least one dosing unit into the resin receiver and mixed in the resin receiver, for example with a suitable mixer.

Настоящее изобретение объясняется ниже более подробно со ссылкой на несколько примеров осуществления.The present invention is explained below in more detail with reference to several embodiments.

Пример осуществления 1Embodiment 1

На производственной линии, которая работает со скоростью подачи 25 м/мин, укладывали с валика декоративную бумагу (граммаж: 80 г/м2). В устройстве для нанесения декоративную бумагу затем покрывали сверху с помощью трибостатических пистолетов порошком меламиновой смолы в количестве 70 г/м2. Порошок меламиновой смолы содержал обычные вспомогательные вещества, такие как отвердители, антиадгезивы и т.д. Затем порошок подплавляли с использованием инфракрасного излучения.On a production line which operates at a feed rate of 25 m/min, decorative paper (grammage: 80 g/m 2 ) was laid down from a roller. In the applicator, the decorative paper was then top coated with 70 g/m 2 melamine resin powder using tribo guns. The melamine resin powder contained common auxiliary substances such as curing agents, release agents, etc. The powder was then melted using infrared radiation.

Затем с помощью щелевого сопла на верхнюю часть наносили дисперсионный материал на основе акрилата в количестве 30 фл/м2 (содержание твердых частиц: приблизительно 50 вес.%). Дисперсионный материал высушивали с помощью ИК-излучателей. Затем поверхность отверждали с помощью эксимерного излучателя (172 нм) под воздействием инертного газа (азота).30 fl/m 2 acrylate-based dispersion material (solids content: approximately 50% by weight) was then applied to the top using a slotted nozzle. The dispersion material was dried using IR emitters. The surface was then cured using an excimer emitter (172 nm) under the influence of an inert gas (nitrogen).

Затем пропитанный слой прессовали поверх носителя в прессе с коротким циклом. На обратной стороне использовали декоративный пропитанный слой без акрилатного покрытия. В качестве носителя применяли древесностружечную плиту толщиной 19 мм. Условиями прессования были: T=200°C, p=40 кг/см2 и t=16 c. Применяли пластину для прессования со структурой бумаги ручной выделки.The impregnated layer was then pressed over the carrier in a short cycle press. On the reverse side, a decorative impregnated layer without an acrylate coating was used. A chipboard 19 mm thick was used as a support. The pressing conditions were: T=200°C, p=40 kg/cm 2 and t=16 s. A pressing plate with a handmade paper texture was used.

После прессования определяли степень блеска (согласно DIN EN ISO 2813:2015-02, угол измерения: 85°), при этом значение составило 3,8 единицы блеска.After pressing, the degree of gloss was determined (according to DIN EN ISO 2813:2015-02, measurement angle: 85°), whereby the value was 3.8 gloss units.

Пропитанный слой, который был пропитан без акрилатного покрытия, при определении степени блеска дал значение 12,3 единицы блеска.The impregnated layer, which was impregnated without the acrylate coating, gave a gloss value of 12.3 gloss units when measured.

Испытатель наносил на поверхность и контрольную область так много отпечатков пальцев, насколько это было возможно. В отличие от контрольной области на поверхности это было невозможно с составом для испытания.The tester applied as many fingerprints to the surface and control area as possible. Unlike the control area on the surface, this was not possible with the test formulation.

Пример осуществления 2Embodiment 2

На производственной линии, которая работает со скоростью подачи 25 м/мин, укладывали с валика бумагу-оверлей (граммаж: 30 г/м2). В распределителе распределяли 20 г корунда/м2 (F230, стандарт FEPA). В устройстве для нанесения бумагу-оверлей затем покрывали сверху с помощью трибостатических пистолетов порошком меламиновой смолы в количестве 20 г/м2. Порошок меламиновой смолы содержал обычные вспомогательные вещества, такие как отвердители, антиадгезивы и т.д. Затем порошок подплавляли с использованием инфракрасного излучения.An overlay paper (grammage: 30 g/m 2 ) was laid from a roller on a production line that was running at a feed speed of 25 m/min. 20 g of corundum/m 2 (F230, FEPA standard) were distributed in the distributor. In the applicator, the overlay paper was then top coated with 20 g/m 2 melamine resin powder using tribo guns. The melamine resin powder contained common auxiliary substances such as curing agents, release agents, etc. The powder was then melted using infrared radiation.

Затем порошок меламиновой смолы в количестве 80 г/м2 наносили на обратную часть также с помощью устройства для нанесения, которое, в свою очередь, работает с трибостатическими пистолетами, и обеспечивали загустение с помощью ИК-излучателей. Порошок меламиновой смолы содержал обычные вспомогательные вещества, такие как отвердители, антиадгезивы и т.д.Then melamine resin powder in the amount of 80 g/m 2 was applied to the backside also by means of an applicator, which, in turn, works with tribostatic guns, and thickened with IR emitters. The melamine resin powder contained common auxiliary substances such as curing agents, release agents, etc.

Затем с помощью щелевого сопла на эту меламиновую смолу на нижней стороне наносили дисперсионный материал на основе акрилата в количестве 30 фл/м2 (содержание твердых частиц: приблизительно 50 вес.%). Дисперсионный материал высушивали с помощью ИК-излучателей. Затем поверхность отверждали с помощью эксимерного излучателя (172 нм) под воздействием инертного газа.The acrylate-based dispersion material was then applied to this melamine resin on the underside using a slotted nozzle in an amount of 30 fl/m 2 (solids content: approximately 50% by weight). The dispersion material was dried using IR emitters. The surface was then cured using an excimer emitter (172 nm) under the influence of an inert gas.

Пропитанный верхний слой с акрилатным покрытием, обращенным вверх, затем прижимали к HDF толщиной 7 мм в прессе с коротким циклом на декоративном пропитанном слое с верхней стороны и стабилизирующем слое с нижней стороны. Условиями прессования были: T=200°C, p=40 кг/см2 и t=16 c. Применяли пластину для прессования со структурой бумаги ручной выделки.The impregnated top layer, with the acrylate coating facing upwards, was then pressed against a 7 mm thick HDF in a short cycle press on the decorative impregnated layer on the top side and the stabilizing layer on the bottom side. The pressing conditions were: T=200°C, p=40 kg/cm 2 and t=16 s. A pressing plate with a handmade paper texture was used.

После прессования определяли степень блеска (согласно DIN EN ISO 2813:2015-02, угол измерения: 85°), при этом значение составило 3,8 единицы блеска. В качестве эталона прессование с пропитанным верхним слоем, который был получен без акрилатного покрытия, дало значение 12,3 единицы блеска при определении степени блеска.After pressing, the degree of gloss was determined (according to DIN EN ISO 2813:2015-02, measurement angle: 85°), whereby the value was 3.8 gloss units. As a reference, pressing with an impregnated top layer, which was obtained without an acrylate coating, gave a value of 12.3 gloss units when determining the degree of gloss.

Испытатель наносил на поверхность и контрольную область так много отпечатков пальцев, насколько это было возможно. В отличие от контрольной области на поверхности это было невозможно с составом для испытания.The tester applied as many fingerprints to the surface and control area as possible. Unlike the control area on the surface, this was not possible with the test composition.

При испытании устойчивости к истиранию в соответствии с DIN EN 13329, 2016-08 был обнаружен класс прочности 32.In an abrasion resistance test according to DIN EN 13329, 2016-08, strength class 32 was found.

Пример осуществления 3Embodiment 3

На производственной линии HDF толщиной 8 мм отделяли, очищали от пыли с помощью щеток и затем транспортировали роликовыми транспортерами (система подачи: 30 м/мин). В устройстве для нанесения их затем покрывали с помощью трибостатических пистолетов порошком меламиновой смолы в количестве 25 г/м2. Порошок меламиновой смолы содержал обычные вспомогательные вещества, такие как отвердители, антиадгезивы и т.д. Затем порошок подплавляли с использованием инфракрасного излучения.On the production line, HDF with a thickness of 8 mm was separated, dusted with brushes, and then transported by roller conveyors (feeding system: 30 m/min). In the applicator, they were then coated with 25 g/m 2 melamine resin powder using tribostatic guns. The melamine resin powder contained common auxiliary substances such as curing agents, release agents, etc. The powder was then melted using infrared radiation.

Затем прогрунтованную плиту многократно покрывали цветным грунтовым покрытием с последующим промежуточным высушиванием (циркулирующим воздухом). Цветное грунтовое покрытие представляло собой смесь казеина и пигмента (диоксида титана). Количество нанесения за одно нанесение составляло приблизительно 5 фл/м2. Нанесение повторяли по меньшей мере пять раз. Затем происходило нанесение грунтовки (количество нанесения: 10-20 фл/м2) с высушиванием циркуляционным воздухом. Затем на плиту наносили печать с помощью валиков или цифрового принтера. Количество нанесения краски составляло от 3 до 15 фл/м2. Краску высушивали посредством ИК-излучения или циркуляционного воздуха. Корунд распределяли на оттиск с помощью распределительного устройства (количество нанесения: 20 г корунда/м2, F230, стандарт FEPA). Затем снова наносили порошок меламиновой смолы с помощью трибостатического пистолета (количество нанесения: 60 г/м2). Порошок меламиновой смолы содержал обычные вспомогательные вещества, такие как отвердители, антиадгезивы и т.д. С помощью ИК-излучателя снова обеспечивали загустение этого порошка меламиновой смолы. Порошок меламиновой смолы содержал обычные вспомогательные вещества, такие как отвердители, антиадгезивы и т.д.The primed slab was then repeatedly coated with a colored primer followed by intermediate drying (circulating air). The colored ground coat was a mixture of casein and pigment (titanium dioxide). The amount of application per application was approximately 5 fl/m 2 . Application was repeated at least five times. Then there was the application of the primer (amount of application: 10-20 fl/m 2 ) with drying by circulating air. The board was then printed using rollers or a digital printer. The amount of paint application was from 3 to 15 fl/m 2 . The paint was dried by means of IR radiation or circulating air. Corundum was dispensed onto the impression using a dispenser (application amount: 20 g corundum/m 2 , F230, FEPA standard). Then, the melamine resin powder was applied again with a tribo gun (application amount: 60 g/m 2 ). The melamine resin powder contained common auxiliary substances such as curing agents, release agents, etc. The melamine resin powder was thickened again with an IR emitter. The melamine resin powder contained common auxiliary substances such as curing agents, release agents, etc.

Затем с помощью щелевого сопла на эту меламиновую смолу наносили дисперсионный материал на основе акрилата в количестве 50 фл/м2 (содержание твердых частиц: приблизительно 50 вес.%). Дисперсионный материал высушивали с помощью ИК-излучателей. Затем поверхность отверждали с помощью эксимерного излучателя (172 нм) под воздействием инертного газа.The acrylate-based dispersion material was then applied to this melamine resin using a slotted nozzle in an amount of 50 fl/m 2 (solids content: approximately 50% by weight). The dispersion material was dried using IR emitters. The surface was then cured using an excimer emitter (172 nm) under the influence of an inert gas.

Затем плиту прессовали вместе с пропитанным слоем стабилизирующего слоя в КТ-прессе. Условиями прессования были: T=200°C, p=40 кг/см2 и t=12 c. Применяли пластину для прессования со структурой бумаги ручной выделки. После прессования определяли степень блеска (согласно DIN EN ISO 2813:2015-02, угол измерения: 85°), при этом значение составило 3,4 единицы блеска. Контрольный образец, который был получен без акрилатного покрытия, дал значение 12,9 единицы блеска при определении степени блеска.The board was then pressed together with the impregnated layer of the stabilizer layer in a CT press. The pressing conditions were: T=200°C, p=40 kg/cm 2 and t=12 s. A pressing plate with a handmade paper texture was used. After pressing, the degree of gloss was determined (according to DIN EN ISO 2813:2015-02, measurement angle: 85°), whereby the value was 3.4 gloss units. The control sample, which was obtained without acrylate coating, gave a value of 12.9 units of gloss when determining the degree of gloss.

Испытатель наносил на поверхность и контрольную область так много отпечатков пальцев, насколько это было возможно. В отличие от контрольной области на поверхности это было невозможно с составом для испытания.The tester applied as many fingerprints to the surface and control area as possible. Unlike the control area on the surface, this was not possible with the test formulation.

Последующее проведенное испытание на устойчивость к истиранию в соответствии с DIN EN 15468, август 2018 года, дало в качестве результата класс прочности 32.A subsequent abrasion resistance test carried out in accordance with DIN EN 15468, August 2018, resulted in strength class 32.

Пример осуществления 4Embodiment 4

На производственной линии HDF толщиной 8 мм отделяли, очищали от пыли с помощью щеток и затем транспортировали роликовыми транспортерами (скорость подачи: 30 м/мин). В устройстве для нанесения их затем покрывали с помощью трибостатических пистолетов порошком меламиновой смолы в количестве 25 г/м2. Порошок меламиновой смолы содержал обычные вспомогательные вещества, такие как отвердители, антиадгезивы и т.д. Затем порошок подплавляли с использованием инфракрасного излучения.On the production line, HDF with a thickness of 8 mm was separated, dusted with brushes, and then conveyed by roller conveyors (feed speed: 30 m/min). In the applicator, they were then coated with 25 g/m 2 melamine resin powder using tribostatic guns. The melamine resin powder contained common auxiliary substances such as curing agents, release agents, etc. The powder was then melted using infrared radiation.

Затем прогрунтованную плиту многократно покрывали цветным грунтовым покрытием с последующим промежуточным высушиванием (циркулирующим воздухом). Цветное грунтовое покрытие представляло собой смесь казеина и пигмента (диоксида титана). Количество нанесения за одно нанесение составляло приблизительно 5 фл/м2. Нанесение повторяли по меньшей мере пять раз. Затем происходило нанесение грунтовки (количество нанесения: 10-20 фл/м2 с высушиванием циркуляционным воздухом. Затем на плиту наносили печать с помощью валиков или цифрового принтера. Количество нанесения краски составляло от 3 до 15 фл/м2. Краску высушивали посредством ИК-излучения или циркуляционного воздуха. Затем снова наносили порошок меламиновой смолы с помощью трибостатического пистолета (количество нанесения: 30 г/м2). Порошок меламиновой смолы содержал обычные вспомогательные вещества, такие как отвердители, антиадгезивы и т.п. Снова обеспечивали загустение этого порошка меламиновой смолы с помощью ИК-излучателя. Корунд распределяли на оттиск с помощью распределительного устройства (количество нанесения: 20 г корунда/м2, F230, стандарт FEPA). Затем снова наносили порошок меламиновой смолы с помощью трибостатического пистолета (количество нанесения: 50 г/м2). Порошок меламиновой смолы содержал приблизительно 5 вес.% целлюлозы (Fa. J.

Figure 00000001
Vivapur 302). Порошок меламиновой смолы содержал обычные вспомогательные вещества, такие как отвердители, антиадгезивы и т.п. Снова обеспечивали загустение этого порошка смолы, представляющей собой меламиновую смолу, с помощью ИК-излучателя. Порошок меламиновой смолы содержал обычные вспомогательные вещества, такие как отвердители, антиадгезивы и т.д. Затем с помощью распределительного устройства распределяли стеклянные шарики в количестве приблизительно 8 г/м2 (Fa. Potters, GP 065-90). Новое нанесение порошка меламиновой смолы происходило с помощью трибостатических пистолетов (количество нанесения: 40 г/м2). Также в данном случае в порошке меламиновой смолы содержатся обычные вспомогательные вещества. С помощью ИК-излучателя снова обеспечивали загустение смолы.The primed slab was then repeatedly coated with a colored primer followed by intermediate drying (circulating air). The colored ground coat was a mixture of casein and pigment (titanium dioxide). The amount of application per application was approximately 5 fl/m 2 . Application was repeated at least five times. Then the primer was applied (application amount: 10-20 fl/m 2 with drying by circulating air. Then the board was printed with rollers or a digital printer. The ink application amount was from 3 to 15 fl/m 2 . The paint was dried by IR- radiation or circulating air.Then, the melamine resin powder was again applied with a tribostatic gun (application amount: 30 g/m 2 ) The melamine resin powder contained conventional auxiliary substances such as hardeners, release agents, etc. resin with an IR emitter Corundum was spread onto the impression using a dispenser (application amount: 20 g corundum/m 2 , F230, FEPA standard) Then the melamine resin powder was again applied using a tribostatic gun (application amount: 50 g/m 2 ) The melamine resin powder contained approximately 5% by weight of cellulose (Fa. J.
Figure 00000001
Vivapur 302). The melamine resin powder contained conventional adjuvants such as curing agents, release agents, and the like. This melamine resin resin powder was thickened again with an IR emitter. The melamine resin powder contained common auxiliary substances such as curing agents, release agents, etc. Glass beads were then dispensed using a dispenser in an amount of approximately 8 g/m 2 (Fa. Potters, GP 065-90). The new application of the melamine resin powder took place with tribostatic guns (application amount: 40 g/m 2 ). Also in this case, conventional auxiliaries are contained in the melamine resin powder. With the help of an IR emitter, the resin was thickened again.

Затем с помощью щелевого сопла на эту меламиновую смолу наносили дисперсионный материал на основе акрилата в количестве 40 фл/м2 (содержание твердых частиц: приблизительно 50 вес.%). Дисперсионный материал высушивали с помощью ИК-излучателей. Затем поверхность отверждали с помощью эксимерного излучателя (172 нм) под воздействием инертного газа.The acrylate-based dispersion material was then applied to this melamine resin using a slotted nozzle in an amount of 40 fl/m 2 (solids content: approximately 50% by weight). The dispersion material was dried using IR emitters. The surface was then cured using an excimer emitter (172 nm) under the influence of an inert gas.

Затем плиту прессовали вместе с пропитанным слоем стабилизирующего слоя в КТ-прессе. Условиями прессования были: T=200°C, p=40 кг/см2 и t=15 c. Применяли пластину для прессования со структурой бумаги ручной выделки. После прессования определяли степень блеска (согласно DIN EN ISO 2813: 2015-02, угол измерения: 85°), при этом значение составило 3,8 единицы блеска. Плита, которая была получена без акрилатного покрытия, дала значение 12,0 единицы блеска при определении степени блеска.The board was then pressed together with the impregnated layer of the stabilizer layer in a CT press. The pressing conditions were: T=200°C, p=40 kg/cm 2 and t=15 s. A pressing plate with a handmade paper texture was used. After pressing, the degree of gloss was determined (according to DIN EN ISO 2813: 2015-02, measurement angle: 85°), and the value was 3.8 gloss units. The slab, which was obtained without an acrylate coating, gave a value of 12.0 units of gloss when determining the degree of gloss.

Испытатель наносил на поверхность и контрольную область так много отпечатков пальцев, насколько это было возможно. В отличие от контрольной области на поверхности это было невозможно с составом для испытания.The tester applied as many fingerprints to the surface and control area as possible. Unlike the control area on the surface, this was not possible with the test composition.

Последующее проведенное испытание на устойчивость к истиранию в соответствии с DIN EN 15468, август 2018 года, дало в качестве результата класс прочности 32.A subsequent abrasion resistance test carried out in accordance with DIN EN 15468, August 2018, resulted in strength class 32.

Пример осуществления 5Embodiment 5

На производственной линии HDF толщиной 8 мм отделяли, очищали от пыли с помощью щеток и затем транспортировали роликовыми транспортерами (система подачи: 30 м/мин). В устройстве для нанесения их затем покрывали с помощью трибостатических пистолетов порошком меламиновой смолы в количестве 25 г/м2. Порошок меламиновой смолы содержал обычные вспомогательные вещества, такие как отвердители, антиадгезивы и т.д. Кроме того, смола содержала 3 вес.% углеродных нанотрубок. Затем порошок подплавляли с использованием инфракрасного излучения.On the production line, HDF with a thickness of 8 mm was separated, dusted with brushes, and then transported by roller conveyors (feeding system: 30 m/min). In the applicator, they were then coated with 25 g/m 2 melamine resin powder using tribostatic guns. The melamine resin powder contained common auxiliary substances such as curing agents, release agents, etc. In addition, the resin contained 3% by weight of carbon nanotubes. The powder was then melted using infrared radiation.

Затем прогрунтованную плиту многократно покрывали цветным грунтовым покрытием с последующим промежуточным высушиванием (циркулирующим воздухом). Цветное грунтовое покрытие представляло собой смесь казеина и пигмента (диоксида титана). Количество нанесения за одно нанесение составляло приблизительно 5 фл/м2. Нанесение повторяли по меньшей мере пять раз. Затем происходило нанесение грунтовки (количество нанесения: 10-20 фл/м2) с высушиванием циркуляционным воздухом. Затем на плиту наносили печать с помощью валиков или цифрового принтера. Количество нанесения краски составляло от 3 до 15 фл/м2. Краску высушивали посредством ИК-излучения или циркуляционного воздуха. Затем снова наносили порошок меламиновой смолы с помощью трибостатического пистолета (количество нанесения: 30 г/м2). Порошок меламиновой смолы содержал обычные вспомогательные вещества, такие как отвердители, антиадгезивы и т.д. С помощью ИК-излучателя снова обеспечивали загустение этого порошка меламиновой смолы. Корунд распределяли на оттиск с помощью распределительного устройства (количество нанесения: 20 г корунда/м2, F230). Затем снова наносили порошок меламиновой смолы с помощью трибостатического пистолета (количество нанесения: 50 г/м2). Порошок меламиновой смолы содержал приблизительно 5 вес.% целлюлозы (Fa. J.

Figure 00000001
Vivapur 302). С помощью ИК-излучателя снова обеспечивали загустение этого порошка меламиновой смолы. Порошок меламиновой смолы содержал обычные вспомогательные вещества, такие как отвердители, антиадгезивы и т.д. Затем с помощью распределительного устройства распределяли стеклянные шарики в количестве приблизительно 8 г/м2 (Fa. Potters, GP 065-90). Новое нанесение порошка меламиновой смолы происходило с помощью трибостатических пистолетов (количество нанесения: 40 г/м2). Также в данном случае в порошке меламиновой смолы содержатся обычные вспомогательные вещества. С помощью ИК-излучателя снова обеспечивали загустение смолы.The primed slab was then repeatedly coated with a colored primer followed by intermediate drying (circulating air). The colored ground coat was a mixture of casein and pigment (titanium dioxide). The amount of application per application was approximately 5 fl/m 2 . Application was repeated at least five times. Then there was the application of the primer (amount of application: 10-20 fl/m 2 ) with drying by circulating air. The board was then printed using rollers or a digital printer. The amount of paint application was from 3 to 15 fl/m 2 . The paint was dried by means of IR radiation or circulating air. Then, the melamine resin powder was applied again with a tribo gun (application amount: 30 g/m 2 ). The melamine resin powder contained common auxiliary substances such as curing agents, release agents, etc. The melamine resin powder was thickened again with an IR emitter. Corundum was dispensed onto the impression using a dispenser (application amount: 20 g corundum/m 2 , F230). Then, the melamine resin powder was applied again with a tribo gun (application amount: 50 g/m 2 ). The melamine resin powder contained approximately 5% by weight of cellulose (Fa. J.
Figure 00000001
Vivapur 302). The melamine resin powder was thickened again with an IR emitter. The melamine resin powder contained common auxiliary substances such as curing agents, release agents, etc. Glass beads were then dispensed using a dispenser in an amount of approximately 8 g/m 2 (Fa. Potters, GP 065-90). The new application of the melamine resin powder took place with tribostatic guns (application amount: 40 g/m 2 ). Also in this case, conventional auxiliaries are contained in the melamine resin powder. With the help of an IR emitter, the resin was thickened again.

Затем с помощью щелевого сопла на эту меламиновую смолу наносили дисперсионный материал на основе акрилата в количестве 40 фл/м2 (содержание твердых частиц: приблизительно 50 вес.%). Дисперсионный материал высушивали с помощью ИК-излучателей. Затем поверхность отверждали с помощью эксимерного излучателя (172 нм) под воздействием инертного газа.The acrylate-based dispersion material was then applied to this melamine resin using a slotted nozzle in an amount of 40 fl/m 2 (solids content: approximately 50% by weight). The dispersion material was dried using IR emitters. The surface was then cured using an excimer emitter (172 nm) under the influence of an inert gas.

Затем плиту прессовали вместе с пропитанным слоем стабилизирующего слоя в КТ-прессе. Условиями прессования были: T=200°C, p=40 кг/см2 и t=15 c. Применяли пластину для прессования со структурой бумаги ручной выделки. После прессования определяли степень блеска (согласно DIN EN ISO 2813:2015-02, угол измерения: 85°), при этом значение составило 3,8 единицы блеска. Плита, которая была получена без акрилатного покрытия, дала значение 12,0 единицы блеска при определении степени блеска.The board was then pressed together with the impregnated layer of the stabilizer layer in a CT press. The pressing conditions were: T=200°C, p=40 kg/cm 2 and t=15 s. A pressing plate with a handmade paper texture was used. After pressing, the degree of gloss was determined (according to DIN EN ISO 2813:2015-02, measurement angle: 85°), whereby the value was 3.8 gloss units. The slab, which was obtained without an acrylate coating, gave a value of 12.0 units of gloss when determining the degree of gloss.

Испытатель наносил на поверхность и контрольную область так много отпечатков пальцев, насколько это было возможно. В отличие от контрольной области на поверхности это было невозможно с составом для испытания.The tester applied as many fingerprints to the surface and control area as possible. Unlike the control area on the surface, this was not possible with the test formulation.

Последующее проведенное испытание на устойчивость к истиранию в соответствии с DIN EN 15468, август 2018 года, дало в качестве результата класс прочности 32. Измерение сопротивления поверхности дало значение 7,8×108 Ом.A subsequent abrasion resistance test carried out in accordance with DIN EN 15468, August 2018, resulted in strength class 32. The measurement of the surface resistance gave a value of 7.8×10 8 ohm.

Claims (57)

1. Способ получения материала-основы для мебельной промышленности, напольных покрытий, облицовки стен и потолков, снабженного по меньшей мере одним матированным покрытием, препятствующим сохранению отпечатков пальцев, при этом материал-основа представляет собой слой бумаги или плиту на основе древесного материала, включающий этапы:1. A method for producing a base material for the furniture industry, flooring, wall and ceiling cladding, provided with at least one matte coating that prevents the preservation of fingerprints, while the base material is a layer of paper or a board based on wood material, including the steps : - нанесения по меньшей мере одного слоя из по меньшей мере одной порошкообразной формальдегидной смолы на по меньшей мере одну сторону материала-основы;- applying at least one layer of at least one formaldehyde resin powder to at least one side of the base material; - плавления по меньшей мере одного нанесенного слоя из порошкообразной формальдегидной смолы;- melting at least one deposited layer of powdered formaldehyde resin; - нанесения по меньшей мере одного дисперсионного материала, содержащего акрилат, на подплавленный слой формальдегидной смолы и- applying at least one dispersion material containing acrylate to the sub-melted layer of formaldehyde resin and - высушивания и отверждения слоистой структуры.- drying and curing of the layered structure. 2. Способ по п. 1, отличающийся тем, что слой бумаги представляет собой декоративный слой бумаги или слой бумаги-оверлей.2. The method according to claim 1, characterized in that the paper layer is a decorative paper layer or an overlay paper layer. 3. Способ по п. 1, отличающийся тем, что плита на основе древесного материала представляет собой древесноволокнистую плиту средней плотности (MDF), древесноволокнистую плиту высокой плотности (HDF) или ориентированно-стружечную плиту (OSB), клееную плиту или плиту на основе древесно-пластикового композита (WPC).3. The method of claim 1, wherein the wood based board is medium density fibreboard (MDF), high density fibreboard (HDF) or oriented strand board (OSB), glued board or wood based board. - plastic composite (WPC). 4. Способ по любому из предыдущих пунктов, отличающийся тем, что на материал-основу наносят порошкообразную формальдегидную смолу посредством электростатического заряда.4. Method according to any one of the preceding claims, characterized in that powdered formaldehyde resin is applied to the base material by means of an electrostatic charge. 5. Способ по любому из предыдущих пунктов, отличающийся тем, что порошкообразная формальдегидная смола представляет собой карбамидную смолу, меламиновую смолу или фенольную смолу, особенно предпочтительно меламиноформальдегидную смолу.5. Method according to any one of the preceding claims, characterized in that the powdered formaldehyde resin is a carbamide resin, a melamine resin or a phenolic resin, particularly preferably a melamine-formaldehyde resin. 6. Способ по любому из предыдущих пунктов, отличающийся тем, что порошкообразная формальдегидная смола содержит пигменты, электропроводящие вещества и/или целлюлозу.6. Method according to any one of the preceding claims, characterized in that the formaldehyde resin powder contains pigments, electrically conductive substances and/or cellulose. 7. Способ по любому из предыдущих пунктов, отличающийся тем, что включает следующие этапы:7. The method according to any of the previous paragraphs, characterized in that it includes the following steps: - нанесение по меньшей мере одного первого слоя из по меньшей мере одной порошкообразной формальдегидной смолы на по меньшей мере одну сторону материала-основы и плавление по меньшей мере одного нанесенного слоя из порошкообразной смолы;applying at least one first layer of at least one powdered formaldehyde resin to at least one side of the base material and melting at least one applied layer of powdered resin; - нанесение по меньшей мере одного декоративного слоя на по меньшей мере один подплавленный слой формальдегидной смолы посредством способа прямой печати;- applying at least one decorative layer to at least one sub-melted layer of formaldehyde resin by means of a direct printing method; - нанесение по меньшей мере одного дополнительного второго слоя из по меньшей мере одной порошкообразной формальдегидной смолы на по меньшей мере один декоративный слой с нанесенной печатью;applying at least one additional second layer of at least one formaldehyde resin powder to at least one printed decorative layer; - плавление по меньшей мере одного слоя, нанесенного на декоративный слой, из порошкообразной формальдегидной смолы;- melting at least one layer deposited on the decorative layer of powdered formaldehyde resin; - нанесение по меньшей мере одного дисперсионного материала, содержащего акрилат, на подплавленный слой формальдегидной смолы и- applying at least one dispersion material containing acrylate on the melted layer of formaldehyde resin and - высушивание и отверждение слоистой структуры.- drying and curing of the layered structure. 8. Способ по п. 7, отличающийся тем, что перед нанесением печати на подплавленный слой порошка формальдегидной смолы наносят по меньшей мере одно грунтовое покрытие.8. The method according to claim 7, characterized in that at least one primer coat is applied to the melted layer of formaldehyde resin powder before printing. 9. Способ по п. 8, отличающийся тем, что по меньшей мере одно грунтовое покрытие содержит казеин, кукурузный крахмал или соевый белок.9. The method according to claim 8, characterized in that at least one ground coating contains casein, corn starch or soy protein. 10. Способ по п. 8 или 9, отличающийся тем, что перед нанесением печати, в частности, на по меньшей мере одно грунтовое покрытие наносят по меньшей мере один грунтовочный слой.10. Method according to claim 8 or 9, characterized in that at least one primer layer is applied to the at least one primer coat before printing, in particular. 11. Способ по любому из пп. 7-10, отличающийся тем, что на декоративном слое или на подплавленных слоях порошка формальдегидной смолы равномерно распределяют износостойкие частицы.11. The method according to any one of paragraphs. 7-10, characterized in that wear-resistant particles are evenly distributed on the decorative layer or on the melted layers of the formaldehyde resin powder. 12. Способ по п. 11, отличающийся тем, что по меньшей мере один дополнительный третий слой из по меньшей мере одной порошкообразной формальдегидной смолы наносят, в частности, на слой из износостойких частиц.12. Method according to claim 11, characterized in that at least one additional third layer of at least one formaldehyde resin powder is applied, in particular, to the layer of wear-resistant particles. 13. Способ по п. 12, отличающийся тем, что стеклянные шарики распределяют, в частности, на по меньшей мере одном дополнительном третьем подплавленном слое порошка формальдегидной смолы.13. Method according to claim 12, characterized in that the glass beads are distributed, in particular, on at least one additional third subfused layer of formaldehyde resin powder. 14. Способ по п. 13, отличающийся тем, что по меньшей мере один дополнительный четвертый слой из по меньшей мере одной порошкообразной формальдегидной смолы наносят, в частности, на слой из стеклянных шариков.14. Method according to claim 13, characterized in that at least one additional fourth layer of at least one formaldehyde resin powder is applied, in particular, to a layer of glass beads. 15. Способ по любому из предыдущих пунктов, отличающийся тем, что по меньшей мере один дисперсионный материал, содержащий акрилат, содержит отверждаемый излучением лак, содержащий акрилат, в частности, выбранный из сложного-полиэфир(мет)акрилата, простого-полиэфир(мет)акрилата, эпокси(мет)акрилата или уретан(мет)акрилата.15. Method according to any one of the preceding claims, characterized in that at least one acrylate-containing dispersion material comprises a radiation-curable lacquer containing acrylate, in particular selected from polyester(meth)acrylate, polyether(meth) acrylate, epoxy(meth)acrylate or urethane(meth)acrylate. 16. Способ по любому из предыдущих пунктов, отличающийся тем, что по меньшей мере один дисперсионный материал, содержащий акрилат, отверждают под воздействием инертного газа после нанесения с применением УФ-излучателя при значениях длины волны от 120 до 350 нм, предпочтительно от 150 до 250 нм, особенно предпочтительно от 170 до 200 нм.16. A method according to any of the preceding claims, characterized in that at least one dispersion material containing acrylate is cured under the influence of an inert gas after application using a UV emitter at wavelengths from 120 to 350 nm, preferably from 150 to 250 nm, particularly preferably from 170 to 200 nm. 17. Способ по любому из предыдущих пунктов, отличающийся тем, что слоистую структуру прессуют в прессе с коротким циклом.17. A method according to any one of the preceding claims, characterized in that the layered structure is pressed in a short cycle press. 18. Способ по любому из пп. 1-6, 15-17, отличающийся тем, что включает следующие этапы:18. The method according to any one of paragraphs. 1-6, 15-17, characterized in that it includes the following steps: - нанесение по меньшей мере одного первого слоя из по меньшей мере одной порошкообразной формальдегидной смолы на по меньшей мере одну сторону слоя бумаги и плавление по меньшей мере одного нанесенного слоя из порошкообразной формальдегидной смолы;applying at least one first layer of at least one formaldehyde resin powder to at least one side of the paper layer and melting at least one applied layer of formaldehyde resin powder; - нанесение по меньшей мере одного дисперсионного материала, содержащего акрилат, на подплавленный слой формальдегидной смолы и- applying at least one dispersion material containing acrylate on the melted layer of formaldehyde resin and - высушивание и отверждение слоистой структуры.- drying and curing of the layered structure. 19. Слой бумаги, получаемый в способе по любому из предыдущих пунктов, отличающийся тем, что степень блеска составляет менее 10.19. A layer of paper obtained in the method according to any one of the preceding paragraphs, characterized in that the degree of gloss is less than 10. 20. Слой бумаги по п. 19, отличающийся тем, что указанный слой бумаги представляет собой декоративный слой бумаги или слой бумаги-оверлей.20. A paper layer according to claim 19, characterized in that said paper layer is a decorative paper layer or an overlay paper layer. 21. Слой бумаги по п. 19 или 20, отличающийся тем, что степень блеска указанного слоя бумаги составляет менее 8, предпочтительно менее 5.21. Paper layer according to claim 19 or 20, characterized in that the degree of gloss of said paper layer is less than 8, preferably less than 5. 22. Способ по любому из пп. 1-6, 15-17, отличающийся тем, что включает следующие этапы:22. The method according to any one of paragraphs. 1-6, 15-17, characterized in that it includes the following steps: - нанесение по меньшей мере одного первого слоя из по меньшей мере одной порошкообразной формальдегидной смолы на по меньшей мере одну сторону плиты на основе древесного материала и плавление по меньшей мере одного нанесенного слоя из порошкообразной формальдегидной смолы;applying at least one first layer of at least one formaldehyde resin powder to at least one side of the wood based board and melting the at least one applied layer of formaldehyde resin powder; - нанесение по меньшей мере одного грунтового покрытия на подплавленный слой порошка формальдегидной смолы;- applying at least one primer coating on the sub-melted layer of formaldehyde resin powder; - нанесение по меньшей мере одного грунтовочного слоя на по меньшей мере одно грунтовое покрытие;- applying at least one primer layer to at least one primer coat; - нанесение по меньшей мере одного декоративного слоя посредством способа прямой печати;- applying at least one decorative layer by means of a direct printing method; - распределение износостойких частиц;- distribution of wear-resistant particles; - нанесение по меньшей мере одного дополнительного слоя из по меньшей мере одной порошкообразной формальдегидной смолы на по меньшей мере один слой из износостойких частиц и плавление нанесенного слоя из порошкообразной формальдегидной смолы;- applying at least one additional layer of at least one powdered formaldehyde resin to at least one layer of wear-resistant particles and melting the applied layer of powdered formaldehyde resin; - нанесение, высушивание и отверждение по меньшей мере одного дисперсионного материала, содержащего акрилат, на подплавленном слое формальдегидной смолы и- applying, drying and curing at least one dispersion material containing acrylate on the subfused layer of formaldehyde resin and - прессование слоистой структуры.- pressing a layered structure. 23. Способ по любому из пп. 1-6, 15-17, отличающийся тем, что включает следующие этапы:23. The method according to any one of paragraphs. 1-6, 15-17, characterized in that it includes the following steps: - нанесение по меньшей мере одного первого слоя из по меньшей мере одной порошкообразной формальдегидной смолы на по меньшей мере одну сторону плиты на основе древесного материала и плавление по меньшей мере одного нанесенного слоя из порошкообразной формальдегидной смолы;applying at least one first layer of at least one formaldehyde resin powder to at least one side of the wood based board and melting the at least one applied layer of formaldehyde resin powder; - нанесение по меньшей мере одного грунтового покрытия на подплавленный первый слой порошка формальдегидной смолы;- applying at least one ground coat on the melted first layer of formaldehyde resin powder; - нанесение по меньшей мере одного грунтовочного слоя на по меньшей мере одно грунтовое покрытие;- applying at least one primer layer to at least one primer coat; - нанесение по меньшей мере одного декоративного слоя посредством способа прямой печати;- applying at least one decorative layer by means of a direct printing method; - нанесение по меньшей мере одного дополнительного второго слоя из по меньшей мере одной порошкообразной формальдегидной смолы на по меньшей мере один декоративный слой с нанесенной печатью и плавление по меньшей мере одного второго слоя из порошкообразной формальдегидной смолы, нанесенного на декоративный слой;applying at least one additional second layer of at least one formaldehyde resin powder to at least one printed decorative layer and melting at least one second layer of formaldehyde resin powder applied to the decorative layer; - распределение износостойких частиц;- distribution of wear-resistant particles; - нанесение по меньшей мере одного дополнительного третьего слоя из по меньшей мере одной порошкообразной формальдегидной смолы на по меньшей мере один слой из износостойких частиц и плавление нанесенного третьего слоя из порошкообразной формальдегидной смолы;- applying at least one additional third layer of at least one powdered formaldehyde resin to at least one layer of wear-resistant particles and melting the applied third layer of powdered formaldehyde resin; - распределение стеклянных шариков на по меньшей мере одном третьем подплавленном слое порошка формальдегидной смолы;- the distribution of glass beads on at least one third subfused layer of formaldehyde resin powder; - нанесение по меньшей мере одного дополнительного четвертого слоя из по меньшей мере одной порошкообразной формальдегидной смолы на слой из стеклянных шариков и плавление нанесенного четвертого слоя из порошкообразной формальдегидной смолы;- applying at least one additional fourth layer of at least one powdered formaldehyde resin to the layer of glass beads and melting the applied fourth layer of powdered formaldehyde resin; - нанесение, высушивание и отверждение по меньшей мере одного дисперсионного материала, содержащего акрилат, на подплавленном слое смолы и- applying, drying and curing at least one dispersion material containing acrylate on the melted resin layer and - прессование слоистой структуры.- pressing a layered structure. 24. Плита на основе древесного материала, получаемая в способе по любому из пп. 1-17, 22, 23, отличающаяся тем, что степень блеска составляет менее 10.24. Board based on wood material obtained in the method according to any one of paragraphs. 1-17, 22, 23, characterized in that the degree of gloss is less than 10. 25. Плита на основе древесного материала по п. 24, отличающаяся тем, что степень блеска указанной плиты на основе древесного материала составляет менее 8, предпочтительно менее 5.25. Wood-based board according to claim 24, characterized in that said wood-based board has a gloss level of less than 8, preferably less than 5.
RU2021132820A 2019-05-13 2020-05-06 Method for obtaining matted base material with an anti-fingerprint coating RU2792211C1 (en)