RU2453492C1 - Method of fabricating jack-pad and said jack-pad - Google Patents

Method of fabricating jack-pad and said jack-pad Download PDF

Info

Publication number
RU2453492C1
RU2453492C1 RU2010151651/11A RU2010151651A RU2453492C1 RU 2453492 C1 RU2453492 C1 RU 2453492C1 RU 2010151651/11 A RU2010151651/11 A RU 2010151651/11A RU 2010151651 A RU2010151651 A RU 2010151651A RU 2453492 C1 RU2453492 C1 RU 2453492C1
Authority
RU
Russia
Prior art keywords
layers
points
distance
tape
rows
Prior art date
Application number
RU2010151651/11A
Other languages
Russian (ru)
Inventor
Евгений Федорович Харченко (RU)
Евгений Федорович Харченко
Владимир Александрович Анискович (RU)
Владимир Александрович Анискович
Николай Александрович Зеленов (RU)
Николай Александрович Зеленов
Владимир Иванович Губин (RU)
Владимир Иванович Губин
Original Assignee
Общество с ограниченной ответственностью Научно-производственное предприятие "АРМОКОМ-ЦЕНТР"
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Общество с ограниченной ответственностью Научно-производственное предприятие "АРМОКОМ-ЦЕНТР" filed Critical Общество с ограниченной ответственностью Научно-производственное предприятие "АРМОКОМ-ЦЕНТР"
Priority to RU2010151651/11A priority Critical patent/RU2453492C1/en
Application granted granted Critical
Publication of RU2453492C1 publication Critical patent/RU2453492C1/en

Abstract

FIELD: transport.
SUBSTANCE: jacket 4 made up of 5-15 layers of continuous high-strength fabric tape is wound on tight chamber 2 shaped to equilateral triangle and made of thin-wall elasto-plastic material with union 4 at its angle. Width of said tape corresponds to height of chamber triangle. Tape creases are made at 60° to tape lengthwise edges to wrap union 3. Adjacent layers are jointed together in the area of circle 10 inscribed in triangle by point adhesive elastoplastic joints 11. Layers 5 are additionally secured at angles of triangular jacket. Jack-pad is produced in implementation of said method.
EFFECT: reliable and simple design.
18 cl, 8 dwg

Description

Изобретение относится к средствам подъема грузов, пневмо- и гидроподъемникам, домкратам и т.д.The invention relates to a means of lifting goods, pneumatic and hydraulic hoists, jacks, etc.

Известен пневматический подъемник по патенту RU 2048415 С1, МПК7 В66В 9/04 от 23.07.91.Known pneumatic lift according to patent RU 2048415 C1, IPC 7 BV 9/04 from 07/23/91.

Известно подъемное устройство по SU 1114610, 1982 г., МПК7 В66В 9/04 от 23.07.91.Known lifting device according to SU 1114610, 1982, IPC 7 V66V 9/04 from 07/23/91.

Известно подъемное устройство по SU 670500 А1 от 17.02.1978 г., МПК7 В63С 9/00, содержащее герметичную емкость из эластичного материала и оболочку из высокопрочных полотнищ, окантованных по периметру.Known lifting device according to SU 670500 A1 from 02.17.1978, IPC 7 В63С 9/00, containing a sealed container of elastic material and a shell of high strength panels, edged around the perimeter.

Известно подъемное устройство по патенту US 4134475, 1979, В66F 7/16.Known lifting device according to patent US 4134475, 1979, B66F 7/16.

Известно подъемное устройство по патенту WO 2010011214 А1 от 23.07.2008 г., В66В 9/04.Known lifting device according to patent WO 2010011214 A1 from 07/23/2008, BVB 9/04.

Известно подъемное устройство по патенту RU 2245295 С2, В66F 3/24, содержащее камеру из гибкого высокопрочного материала, в которую подается рабочий агент под давлением.Known lifting device according to patent RU 2245295 C2, B66F 3/24, containing a chamber of flexible high-strength material, into which a working agent is supplied under pressure.

Известен пневматический домкрат по патенту RU 2322383 С1 от 10.10. 2006 г., В66F 3/24, содержащий прямоугольную камеру из упруго-эластичного материала, в которую подается рабочий агент под давлением, и чехол, выполненный из двух слоев, материал которых армирован преимущественно во взаимно перпендикулярных направлениях.Known pneumatic jack according to patent RU 2322383 C1 from 10.10. 2006, B66F 3/24, containing a rectangular chamber of elastic material into which a working agent is supplied under pressure, and a cover made of two layers, the material of which is reinforced mainly in mutually perpendicular directions.

Известные решения определяют общий уровень техники и не являются особо релевантными, поэтому предлагаемым решением устраняются недостатки общего известного уровня техники.Known solutions determine the general level of technology and are not particularly relevant, therefore, the proposed solution eliminates the disadvantages of the general prior art.

Недостатками общего известного уровня техники для способа является низкая технологичность изготовления чехла из-за сложного раскроя, сложной намотки при расположении ткани в слоях с равномерным натяжением без гофров и складок с обеспечением заданных размеров, низкая технологичность изготовления чехла, армирующие нити которого воспринимают высокое давление рабочего агента, из-за наличия соединительных швов, требующих высокоточного швейного оборудования, низкая технологичность скрепления соседних контактирующих слоев, которое необходимо для качественной сборки без смещений слоев и должно выполняться без искривлений несущих волокон, по площади максимальных сдвиговых деформаций слоев с учетом работы конструкции по принципу рулонно-тканной емкости давления с минимизацией расхода материала при ее изготовлении, а также с учетом оптимальной прочности скрепления слоев с минимальной жесткостью устройства в нерабочем положении (для складывания при транспортировке и хранении), низкая технологичность скрепления углов и сборки в зоне штуцера для обеспечения надежности работы узла штуцера. Кроме того, недостатком является низкое качество конечного продукта из-за высокой массы камеры и низкого срока службы, а также из-за незащищенности домкрата-подушки от внешних воздействий при хранении и из-за низкого коэффициента трения рабочих поверхностей.The disadvantages of the general prior art for the method is the low manufacturability of the cover due to the complex cutting, the complex winding when the fabric is in layers with uniform tension without corrugations and folds with the specified dimensions, the low manufacturability of the cover, the reinforcing threads of which absorb high pressure of the working agent , due to the presence of connecting seams requiring high-precision sewing equipment, low adaptability of bonding adjacent contact layers, which is not necessary It is suitable for high-quality assembly without displacement of the layers and should be performed without curvature of the bearing fibers, according to the area of maximum shear deformations of the layers, taking into account the design work on the principle of roll-woven pressure capacity with a minimum of material consumption during its manufacture, and also taking into account the optimal bond strength of the layers with a minimum the rigidity of the device in the idle position (for folding during transportation and storage), low adaptability of corner fastening and assembly in the area of the fitting to ensure reliability p fitting node operations. In addition, the disadvantage is the low quality of the final product due to the high weight of the chamber and low life, as well as due to the insecurity of the cushion jack from external influences during storage and due to the low coefficient of friction of the working surfaces.

Недостатками общего известного уровня техники для домкрата-подушки являются низкая надежность работы чехла в условиях применения высокого давления рабочего агента (10 ати и более) из-за наличия в конструкции соединительных швов и связанных с этим искривлений высокопрочных армирующих волокон (например, арамидных), значительно снижающих их характеристики, низкая надежность работы рулонно-тканной емкости, имеющей картину разрушения «размотом» ткани, начиная от наружной кромки, без изменения направления этого «размота», низкая надежность работы чехла из-за неоптимального распределения напряжений в соединениях волокон слоев многослойного чехла при неоптимальном расположении зон скрепления тканой ленты, низкая надежность работы чехла из-за малой площади скрепления ткани в углах и возможности продавливания камеры, а также низкая надежность работы в зоне штуцера. Кроме того, недостатком является низкая надежность работы домкрата-подушки из-за высокой массы камеры и низкого срока ее службы, а также из-за незащищенности домкрата-подушки от внешних воздействий при хранении и из-за низкого коэффициента трения рабочих поверхностей.The disadvantages of the general prior art for a cushion jack are the low reliability of the cover under the conditions of applying high pressure of the working agent (10 ati and more) due to the presence in the design of the joint seams and the associated curvatures of high-strength reinforcing fibers (e.g. aramid) reducing their characteristics, low reliability of the roll-cloth capacity, having a pattern of destruction by "unwinding" the fabric, starting from the outer edge, without changing the direction of this "unwinding", low reliability the work of the cover due to the non-optimal distribution of stresses in the fiber connections of the layers of the multilayer cover with the non-optimal location of the fastening zones of the woven tape, the low reliability of the cover due to the small area of the fastening of the fabric in the corners and the possibility of bursting the camera, as well as the low reliability of operation in the area of the fitting. In addition, the disadvantage is the low reliability of the jack-pillow due to the high mass of the chamber and its low life, as well as due to the insecurity of the jack-pillow from external influences during storage and because of the low coefficient of friction of the working surfaces.

Технической задачей, на решение которой направлены заявляемые изобретения, является создание надежной и высокотехнологичной конструкции домкрата-подушки.The technical problem to which the claimed invention is directed is the creation of a reliable and high-tech design of the pillow jack.

Технический результат для способа, который может быть достигнут при решении технической задачи, заключается в повышении технологичности изготовления чехла за счет значительного упрощения раскроя, упрощения намотки и удобства расположения ткани в слоях с равномерным натяжением без гофров и складок с обеспечением заданных размеров, повышении технологичности изготовления чехла, армирующие нити которого воспринимают высокое давление рабочего агента, за счет исключения соединительных швов, требующих высокоточного швейного оборудования, в повышении технологичности скрепления соседних контактирующих слоев, которое необходимо для качественной сборки без смещений слоев и должно выполняться без искривлений несущих волокон, по площади максимальных сдвиговых деформаций слоев с учетом работы конструкции по принципу рулонно-тканной емкости давления с минимизацией расхода материала при ее изготовлении, а также с учетом оптимальной прочности скрепления слоев с минимальной жесткостью устройства в нерабочем положении (для складывания при транспортировке и хранении), в повышении технологичности скрепления углов, повышении технологичности сборки в зоне штуцера за счет оптимального расположения штуцера вне рабочей зоны устройства с обеспечением надежности работы узла штуцера. Кроме того технический результат заключается в повышении качества конечного продукта за счет снижения массы камеры и повышения срока службы, за счет защиты домкрата-подушки от внешних воздействий при хранении, а также за счет повышения коэффициента трения рабочих поверхностей.The technical result for the method that can be achieved by solving the technical problem is to increase the manufacturability of the cover due to the significant simplification of cutting, simplification of winding and ease of location of the fabric in layers with uniform tension without corrugations and folds with a given size, increasing the manufacturability of the cover whose reinforcing threads absorb high pressure of the working agent, due to the exclusion of connecting seams that require high-precision sewing equipment , to increase the manufacturability of bonding adjacent contacting layers, which is necessary for high-quality assembly without layer displacements and should be performed without curvature of the carrier fibers, over the area of maximum shear deformations of the layers, taking into account the work of the structure on the principle of a roll-woven pressure tank with a minimum of material consumption in its manufacture, and also taking into account the optimal bond strength of the layers with the minimum rigidity of the device in the idle position (for folding during transportation and storage), in increased the technological effectiveness of corner bonding, the technological improvement of assembly in the nozzle area due to the optimal location of the nozzle outside the working area of the device, ensuring the reliability of the nozzle assembly. In addition, the technical result consists in improving the quality of the final product by reducing the weight of the chamber and increasing the service life, by protecting the cushion jack from external influences during storage, as well as by increasing the coefficient of friction of the working surfaces.

Технический результат устройства, который может быть достигнут при решении технической задачи, заключается в повышении надежности работы чехла в условиях применения высокого давления рабочего агента (10 ати и более), за счет исключения из конструкции соединительных швов и связанных с этим искривлений высокопрочных армирующих волокон (например, арамидных), значительно снижающих их характеристики, в повышении надежности работы рулонно-тканной емкости, имеющей картину разрушения «размотом» ткани, за счет изменения направления «размота», повышении надежности работы чехла за счет оптимального расположения зон скрепления тканой ленты, повышении надежности работы чехла за счет увеличения площади их скрепления в углах и отсутствия возможности продавливания камеры в углах, в повышении надежности работы в зоне штуцера, повышении надежности работы чехла за счет оптимального распределения напряжений в соединениях волокон слоев многослойного чехла, работающего как рулонно-тканные емкости давления, с увеличением сдвиговых усилий от внутреннего слоя к наружному, имеющего картину разрушения «размотом» ткани, начиная от наружной кромки, а также в повышении надежности работы домкрата-подушки за счет его защиты от внешних воздействий при хранении и повышении коэффициента трения рабочих поверхностей, кроме того, технический результат заключается в снижении массы изделия.The technical result of the device, which can be achieved by solving the technical problem, is to increase the reliability of the cover in conditions of applying high pressure of the working agent (10 ati and more), by eliminating from the design of the connecting seams and the associated curvatures of high-strength reinforcing fibers (for example , aramid), significantly reducing their characteristics, in improving the reliability of the roll-cloth capacity, which has a pattern of destruction by "unwinding" of the fabric, due to a change in the direction of "unwinding", increasing the reliability of the cover due to the optimal location of the bonding zones of the woven tape, increasing the reliability of the cover due to the increase in the area of bonding in the corners and the lack of the possibility of punching the camera in the corners, increasing the reliability in the area of the fitting, increasing the reliability of the cover due to the optimal voltage distribution in the fiber connections of the layers of a multilayer cover that acts as a roll-woven pressure vessel, with an increase in shear forces from the inner layer to the outer one, which has a pattern well, destruction by unwinding of the fabric, starting from the outer edge, as well as in increasing the reliability of the cushion jack due to its protection from external influences during storage and increasing the friction coefficient of the working surfaces, in addition, the technical result is to reduce the weight of the product.

Поставленная задача с достижением технического результата для способа решается тем, что на герметичную камеру в форме равностороннего треугольника из тонкостенного упруго-эластичного материала со штуцером в ее углу наматывают чехол из 5-15 слоев непрерывной ленты из высокопрочной ткани шириной, соответствующей высоте треугольника камеры, выполняя линии сгиба ленты под углом 60° к продольным краям ленты, обертывая этими краями штуцер, скрепляя соседние слои преимущественно в площади вписанного в треугольник круга точечными клеевыми упруго-эластичными соединениями, с дополнительным скреплением слоев в углах треугольного чехла.The problem with the achievement of the technical result for the method is solved by the fact that a cover of 5-15 layers of a continuous tape of high-strength fabric with a width corresponding to the height of the triangle of the chamber is wound on a sealed chamber in the form of an equilateral triangle of thin-walled elastic material with a fitting in its corner bending lines of the tape at an angle of 60 ° to the longitudinal edges of the tape, wrapping the fitting around these edges, fastening adjacent layers mainly in the area of the circle inscribed in the triangle by point adhesive th-elastic compounds with an additional bonding layer at the corners of the triangular bag.

Углы камеры притупляют радиусом или фаской.The corners of the camera dull with a radius or chamfer.

Скрепление слоев в углах чехла выполняют их пропиткой упруго-эластичной композицией.Bonding layers in the corners of the cover perform their impregnation with an elastic-elastic composition.

Скрепление слоев в углах без штуцера выполняют сквозной прошивкой без повреждения камеры.Bonding layers in the corners without a fitting is done through firmware without damaging the camera.

Скрепление слоев и штуцера выполняют обмоткой пропитанным упруго-эластичной композицией жгутом или пропитанной нитью.The bonding of the layers and the fitting is carried out by winding a bundle impregnated with an elastic-elastic composition or impregnated with a thread.

Клеевые точки располагают рядами в шахматном порядке с расстоянием между рядами, равным расстоянию между точками в рядах, которое определяют исходя из условия расположения между точками 40-120 основных нитей ленты со сдвигом рядов в соседних слоях на (0,4-0,6)l, где l - расстояние между рядами.The glue points are arranged in rows in a checkerboard pattern with the distance between the rows equal to the distance between the points in the rows, which is determined based on the arrangement between the points 40-120 of the main threads of the tape with the rows shifted in adjacent layers by (0.4-0.6) l where l is the distance between the rows.

Клеевые точки выполняют с уменьшением расстояния между точками в процессе намотки от lн до lк=(0,4-0,8)lн, где:Glue points are performed with decreasing the distance between the points during the winding process from l n to l k = (0.4-0.8) l n , where:

- lн - расстояние между точками в начале намотки на первом слое;- l n - the distance between the points at the beginning of the winding on the first layer;

- lк - расстояние между точками в конце намотки на последнем слое.- l to - the distance between the points at the end of the winding on the last layer.

Камеру выполняют из армированного материала объемом, превышающим внутренний объем чехла на 0,4-2,4%.The camera is made of reinforced material with a volume exceeding the internal volume of the cover by 0.4-2.4%.

Домкрат-подушку размещают в защитной прорезиненной оболочке, снабженной снаружи протекторами.The cushion jack is placed in a protective rubberized shell provided with protectors on the outside.

Поставленная задача с достижением технического результата для устройства решается тем, что домкрат-подушка, включающая герметичную камеру в форме равностороннего треугольника из тонкостенного упруго-эластичного материала со штуцером в ее углу, чехол из 5-15 слоев непрерывной ленты из высокопрочной ткани шириной, соответствующей высоте треугольника камеры, намотанный на камеру сгибанием ленты под углом 60° к продольным краям ленты с обертыванием этими краями штуцера, причем соседние слои скреплены преимущественно в площади вписанного в треугольник круга точечными клеевыми упруго-эластичными соединениями с дополнительным скреплением слоев в углах треугольного чехла.The problem is to achieve a technical result for the device is solved by the fact that the jack-pillow, including a sealed chamber in the form of an equilateral triangle of thin-walled elastic material with a fitting in its corner, a cover of 5-15 layers of a continuous tape of high-strength fabric with a width corresponding to the height the triangle of the chamber, wound around the chamber by bending the tape at an angle of 60 ° to the longitudinal edges of the tape with a fitting wrapping around these edges, the adjacent layers being bonded mainly in the area inscribed in circle triangle by point adhesive elastic elastic joints with additional bonding of layers in the corners of a triangular cover.

Углы камеры притуплены радиусом или фаской.The corners of the camera are blunted with a radius or chamfer.

Слои в углах чехла скреплены упруго-эластичной композицией.The layers in the corners of the cover are bonded with an elastic-elastic composition.

Слои в углах без штуцера скреплены сквозной прошивкой без повреждения камеры.Layers in the corners without a fitting are fastened with pass-through firmware without damaging the camera.

Слои и штуцер скреплены обмоткой пропитанным упруго-эластичной композицией жгутом или пропитанной нитью.The layers and the fitting are fastened together with a winding rope impregnated with an elastic-elastic composition or an impregnated thread.

Клеевые точки расположены рядами в шахматном порядке с расстоянием между рядами, равным расстоянию между точками в рядах, которое определено исходя из условия расположения между точками 40-120 основных нитей ленты, со сдвигом рядов в соседних слоях на (0,4-0,6)l, где l - расстояние между рядами.The glue points are arranged in rows in a checkerboard pattern with the distance between the rows equal to the distance between the points in the rows, which is determined based on the arrangement between the points 40-120 of the main threads of the tape, with the rows shifted in adjacent layers by (0.4-0.6) l, where l is the distance between the rows.

Клеевые точки выполнены с уменьшением расстояния между точками в процессе намотки от lн до lк=(0,4-0,8)lн, где:The glue points are made with decreasing the distance between the points during the winding process from l n to l k = (0.4-0.8) l n , where:

- lн - расстояние между точками в начале намотки на первом слое;- l n - the distance between the points at the beginning of the winding on the first layer;

- lк - расстояние между точками в конце намотки на последнем слое.- l to - the distance between the points at the end of the winding on the last layer.

Камера выполнена из армированного материала объемом, превышающим внутренний объем чехла на 0,4-2,4%.The chamber is made of reinforced material with a volume exceeding the internal volume of the cover by 0.4-2.4%.

Домкрат-подушка размещена в защитной прорезиненной оболочке, снабженной снаружи протекторами.The cushion jack is housed in a protective rubberized shell provided with protectors on the outside.

Существенными отличительными от общего известного уровня техники признаками для способа являются следующие признаки:Significant distinguishing features from the general prior art features for the method are the following features:

- на герметичную камеру в форме равностороннего треугольника из тонкостенного упруго-эластичного материала со штуцером в ее углу наматывают чехол из 5-15 слоев непрерывной ленты из высокопрочной ткани шириной, соответствующей высоте треугольника камеры, выполняя линии сгиба ленты под углом 60° к продольным краям ленты, обертывая этими краями штуцер, признаки соответствуют критерию «изобретательский уровень», предусматривают наличие новых операций, новых параметров операций и новую их последовательность, направлены на решение поставленной задачи с достижением технического результата, на повышение технологичности изготовления чехла за счет значительного упрощения раскроя, упрощения намотки и удобства расположения ткани в слоях с равномерным натяжением без гофров и складок с обеспечением заданных размеров;- on a sealed chamber in the form of an equilateral triangle of thin-walled elastic material with a fitting in its corner, a cover of 5-15 layers of a continuous tape of high-strength fabric with a width corresponding to the height of the chamber triangle is wound, performing tape bending lines at an angle of 60 ° to the longitudinal edges of the tape wrapping the fitting around these edges, the signs meet the criterion of "inventive step", provide for the presence of new operations, new parameters of operations and a new sequence of them, aimed at solving second problem with the technical result achievement at improving processability of manufacturing a cover due to a significant simplification of the coating, facilitation and convenience of winding the fabric arrangement in layers with uniform tension without corrugations and creases ensuring predetermined dimensions;

- скрепляя соседние слои преимущественно в площади вписанного в треугольник круга точечными клеевыми упруго-эластичными соединениями с дополнительным скреплением слоев в углах треугольного чехла - признаки соответствуют критерию «изобретательский уровень», предусматривают наличие новых операций и новых параметров операций, направлены на решение поставленной задачи с достижением технического результата на повышение технологичности изготовления чехла, армирующие нити которого воспринимают высокое давление рабочего агента, за счет исключения соединительных швов, требующих высокоточного швейного оборудования, на повышение технологичности скрепления соседних контактирующих слоев, которое необходимо для качественной сборки без смещений слоев и должно выполняться без искривлений несущих волокон, по площади максимальных сдвиговых деформаций слоев, причем данные признаки подтверждены сборкой опытных образцов и функциональной и прочностной отработкой;- bonding adjacent layers mainly in the area of a circle inscribed in a triangle by point adhesive elastic-elastic joints with additional bonding of layers in the corners of a triangular cover - the signs meet the criterion of "inventive step", provide for new operations and new operation parameters aimed at solving the problem with achieving of the technical result to increase the manufacturability of the manufacture of a cover, the reinforcing threads of which perceive high pressure of the working agent, due to elimination of connecting seams that require high-precision sewing equipment to increase the manufacturability of bonding adjacent contact layers, which is necessary for high-quality assembly without displacement of the layers and should be performed without distortion of the bearing fibers, according to the area of maximum shear deformation of the layers, and these signs are confirmed by the assembly of prototypes and functional and strength testing;

- углы камеры притупляют радиусом или фаской - признаки соответствуют критерию «изобретательский уровень», предусматривают наличие новых операций и новую их последовательность, направлены на решение поставленной задачи с достижением технического результата, на повышение технологичности скрепления углов за счет исключения возможности повреждения треугольной камеры;- the corners of the camera are dull with a radius or chamfer - the signs meet the criterion of "inventive step", provide for the presence of new operations and their new sequence, are aimed at solving the problem with achieving a technical result, at increasing the adaptability of corner bonding by eliminating the possibility of damage to the triangular camera;

- скрепление слоев в углах чехла выполняют их пропиткой упруго-эластичной композицией - признаки соответствуют критерию «изобретательский уровень», предусматривают наличие новых операций и новую их последовательность, направлены на решение поставленной задачи с достижением технического результата, на повышение технологичности скрепления углов;- bonding the layers in the corners of the cover is performed by impregnating them with an elastic-elastic composition - the signs meet the criterion of "inventive step", provide for the presence of new operations and a new sequence of them, aimed at solving the problem with achieving a technical result, to improve the manufacturability of bonding corners;

- скрепление слоев в углах без штуцера выполняют сквозной прошивкой без повреждения камеры - признаки соответствуют критерию «изобретательский уровень», предусматривают наличие новых операций и новую их последовательность, направлены на решение поставленной задачи с достижением технического результата, на повышение технологичности прошивки углов за счет исключения возможности повреждения треугольной камеры;- bonding layers in the corners without a fitting is done through firmware without damaging the camera - the signs meet the criterion of "inventive step", provide for new operations and a new sequence of them, aimed at solving the problem with achieving a technical result, to improve the manufacturability of flashing corners by eliminating the possibility damage to the triangular chamber;

- скрепление слоев и штуцера выполняют обмоткой пропитанным упруго-эластичной композицией жгутом или пропитанной нитью - признаки соответствуют критерию «изобретательский уровень», предусматривают наличие новых операций и новую их последовательность, направлены на решение поставленной задачи с достижением технического результата, на повышение технологичности сборки в зоне штуцера за счет оптимального расположения штуцера вне рабочей зоны устройства с обеспечением надежности работы узла штуцера;- the bonding of the layers and the fitting is carried out by winding a bundle soaked in an elastic-elastic composition or impregnated with a thread - the signs meet the criterion of "inventive step", provide for the presence of new operations and their new sequence, aimed at solving the problem with achieving a technical result, to improve the manufacturability of the assembly in the zone the nozzle due to the optimal location of the nozzle outside the working area of the device while ensuring the reliability of the nozzle assembly;

- клеевые точки располагают рядами в шахматном порядке с расстоянием между рядами, равным расстоянию между точками в рядах, которое определяют исходя из условия расположения между точками 40-120 основных нитей ленты, со сдвигом рядов в соседних слоях на (0,4-0,6)l, где l - расстояние между рядами - признаки соответствуют критерию «изобретательский уровень», предусматривают наличие новых операций, новых параметров операций и новую их последовательность, направлены на решение поставленной задачи с достижением технического результата, на повышение технологичности скрепления соседних контактирующих слоев, которое необходимо для качественной сборки без смещений слоев и должно выполняться без искривлений несущих волокон с учетом работы конструкции по принципу рулонно-тканной емкости давления с минимизацией расхода материала при ее изготовлении, а также с учетом оптимальной прочности скрепления слоев с минимальной жесткостью устройства в нерабочем положении (для складывания при транспортировке и хранении), причем данные признаки подтверждены сборкой опытных образцов и функциональной и прочностной отработкой;- adhesive points are arranged in rows in a checkerboard pattern with a distance between the rows equal to the distance between the points in the rows, which is determined based on the arrangement between the points 40-120 of the main threads of the tape, with the rows shifted in adjacent layers by (0.4-0.6 ) l, where l is the distance between the rows - the signs meet the criterion of "inventive step", provide for the presence of new operations, new parameters of operations and their new sequence, are aimed at solving the problem with achieving a technical result, to increase manufacturability of bonding adjacent contacting layers, which is necessary for high-quality assembly without layer displacements and should be performed without curvature of the bearing fibers, taking into account the work of the design on the principle of a roll-woven pressure tank with a minimum of material consumption in its manufacture, and also taking into account the optimal bonding strength of the layers with a minimum the rigidity of the device in the idle position (for folding during transportation and storage), and these signs are confirmed by the assembly of prototypes and functions cial and strength perfecting;

- клеевые точки выполняют с уменьшением расстояния между точками в процессе намотки от lн до lк=(0,4-0,8)lн, где:- adhesive points are performed with decreasing the distance between the points during the winding process from l n to l k = (0.4-0.8) l n , where:

- lн - расстояние между точками в начале намотки на первом слое;- l n - the distance between the points at the beginning of the winding on the first layer;

- lк - расстояние между точками в конце намотки на последнем слое - признаки соответствуют критерию «изобретательский уровень», предусматривают наличие новых операций, новых параметров операций и новую их последовательность, направлены на решение поставленной задачи с достижением технического результата, на повышение технологичности скрепления соседних контактирующих слоев, которое необходимо для качественной сборки без смещений слоев и должно выполняться без искривлений несущих волокон по всей площади всех слоев с учетом оптимальности конструкции с минимизацией расхода материала, так как по условиям прочности и равномерности нагружения армирующих волокон с минимизацией расхода материала скрепление слоев необходимо выполнять только в конце намотки, а по условиям технологичности сборки без смещения слоев необходимо выполнять скрепление всех слоев (данные признаки также подтверждены исследованиями);- l to - the distance between the points at the end of the winding on the last layer - the signs correspond to the criterion of "inventive step", provide for the presence of new operations, new parameters of operations and a new sequence of them, aimed at solving the problem with achieving a technical result, to improve the manufacturability of bonding adjacent contacting layers, which is necessary for high-quality assembly without displacement of the layers and should be performed without distortion of the bearing fibers over the entire area of all layers, taking into account the optimal structural design with minimization of material consumption, since, according to the conditions of strength and uniform loading of reinforcing fibers with minimization of material consumption, the layers need to be bonded only at the end of the winding, and according to the manufacturability conditions without layer shifting, all layers must be bonded (these signs are also confirmed by studies) ;

- камеру выполняют из армированного материала объемом, превышающим внутренний объем чехла на 0,4-2,4% - признаки соответствуют критерию «изобретательский уровень», предусматривают наличие новых операций, новых параметров операций и новую их последовательность, направлены на решение поставленной задачи с достижением технического результата, на повышение технологичности и качества конечного продукта за счет снижения массы камеры и повышения срока службы;- the camera is made of reinforced material with a volume exceeding the internal volume of the cover by 0.4-2.4% - the signs meet the criterion of "inventive step", provide for new operations, new parameters of operations and their new sequence, aimed at solving the problem with achieving the technical result, to improve the manufacturability and quality of the final product by reducing the weight of the chamber and increasing the service life;

- домкрат-подушку размещают в защитной прорезиненной оболочке, снабженной снаружи протекторами - признаки соответствуют критерию «изобретательский уровень», предусматривают наличие новых операций и новую последовательность их выполнения, направлены на решение поставленной задачи с достижением технического результата, на повышение качества конечного продукта за счет защиты домкрата-подушки от внешних воздействий при хранении, а также за счет повышения коэффициента трения рабочих поверхностей.- the jack-pillow is placed in a rubberized protective shell provided with protectors on the outside - the signs meet the criterion of "inventive step", provide for new operations and a new sequence of their implementation, are aimed at solving the problem with achieving a technical result, improving the quality of the final product due to protection jack-pillows from external influences during storage, as well as by increasing the coefficient of friction of the working surfaces.

Существенными отличительными от общего известного уровня техники признаками для устройства являются следующие признаки:Significant distinguishing features from the general prior art features for the device are the following features:

- домкрат-подушка, включающая герметичную камеру в форме равностороннего треугольника из тонкостенного упруго-эластичного материала со штуцером в ее углу, чехол из 5-15 слоев непрерывной ленты из высокопрочной ткани шириной, соответствующей высоте треугольника камеры, намотанный на камеру сгибанием ленты под углом 60° к продольным краям ленты с обертыванием этими краями штуцера - признаки соответствуют критерию «изобретательский уровень», предусматривают наличие новых элементов, их новое взаимное расположение, новое соотношение размеров и новую взаимосвязь элементов, направлены на решение поставленной задачи с достижением технического результата, на повышение надежности работы чехла в условиях применения высокого давления рабочего агента (10 ати и более) за счет исключения из конструкции соединительных швов и связанных с этим искривлений высокопрочных армирующих волокон (например, арамидных), значительно снижающих их характеристики, а также на повышение надежности работы рулонно-тканных емкостей, имеющих картину разрушения «размотом» ткани, за счет изменения направления «размота»;- a cushion jack, including a sealed chamber in the form of an equilateral triangle of thin-walled elastic material with a fitting in its corner, a cover of 5-15 layers of continuous tape of high-strength fabric with a width corresponding to the height of the chamber triangle, wound around the camera by bending the tape at an angle of 60 ° to the longitudinal edges of the tape with a fitting wrapped around these edges - the signs meet the criterion of "inventive step", provide for the presence of new elements, their new relative position, new size ratio c and a new interconnection of elements aimed at solving the problem with achieving a technical result, increasing the reliability of the cover in conditions of applying high pressure of the working agent (10 ati and more) by eliminating from the design of connecting joints and the associated curvature of high-strength reinforcing fibers ( for example, aramid ones), which significantly reduce their characteristics, as well as to increase the reliability of the roll-fabric containers, which have a picture of destruction by "unwinding" of the fabric, due to changes in direction eniya "razmota";

- соседние слои скреплены преимущественно в площади вписанного в треугольник круга точечными клеевыми упруго-эластичными соединениями с дополнительным скреплением слоев в углах треугольного чехла - признаки соответствуют критерию «изобретательский уровень», предусматривают наличие новых элементов, их новое взаимное расположение, новое соотношение размеров и новую взаимосвязь элементов, направлены на решение поставленной задачи с достижением технического результата, на повышение надежности работы чехла за счет оптимального (что подтверждено исследованиями) расположения зон скрепления тканой ленты;- adjacent layers are bonded mainly in the area of the circle inscribed in the triangle by point adhesive elastic elastic joints with additional bonding of the layers in the corners of the triangular cover - the signs meet the criterion of "inventive step", provide for the presence of new elements, their new relative positioning, new size ratio and new relationship elements aimed at solving the problem with achieving a technical result, to increase the reliability of the cover due to the optimal (which con firmed studies) arrangement zones of bonding webbing;

- углы камеры притуплены радиусом или фаской - признаки соответствуют критерию «изобретательский уровень», предусматривают новую форму элементов, направлены на решение поставленной задачи с достижением технического результата, на повышение надежности работы чехла за счет увеличения площади их скрепления в углах;- the corners of the camera are blunted with a radius or bevel - the signs meet the criterion of "inventive step", provide a new form of elements, aimed at solving the problem with achieving a technical result, to increase the reliability of the cover by increasing the area of their bonding in the corners;

- слои в углах чехла скреплены упруго-эластичной композицией - признаки соответствуют критерию «изобретательский уровень», предусматривают новое взаимное расположение элементов и их новую взаимосвязь, направлены на решение поставленной задачи с достижением технического результата, на повышение надежности работы чехла за счет отсутствия возможности продавливания камеры в углах;- the layers in the corners of the cover are fastened with an elastic-elastic composition - the signs meet the criterion of "inventive step", provide for a new mutual arrangement of the elements and their new relationship, are aimed at solving the problem with achieving a technical result, to increase the reliability of the cover due to the inability to push the camera in the corners;

- слои в углах без штуцера скреплены сквозной прошивкой без повреждения камеры - признаки соответствуют критерию «изобретательский уровень», предусматривают новое взаимное расположение элементов и их новую взаимосвязь, направлены на решение поставленной задачи с достижением технического результата, на повышение надежности работы чехла за счет отсутствия возможности продавливания камеры в углах;- layers in the corners without a fitting are fastened with through firmware without damaging the camera - the signs meet the criterion of "inventive step", provide for a new mutual arrangement of elements and their new relationship, aimed at solving the problem with achieving a technical result, to increase the reliability of the cover due to the lack of ability punching the camera in the corners;

- слои и штуцер скреплены обмоткой пропитанным упруго-эластичной композицией жгутом или пропитанной нитью - признаки соответствуют критерию «изобретательский уровень», предусматривают наличие новых элементов и их новую взаимосвязь, направлены на решение поставленной задачи с достижением технического результата, на повышение надежности работы в зоне штуцера;- the layers and the nozzle are fastened together with a winding impregnated with an elastic-elastic composition with a tow or impregnated with a thread - the signs meet the criterion of "inventive step", provide for the presence of new elements and their new relationship, aimed at solving the problem with achieving a technical result, to increase the reliability of work in the nozzle area ;

- клеевые точки расположены рядами в шахматном порядке с расстоянием между рядами, равным расстоянию между точками в рядах, которое определено исходя из условия расположения между точками 40-120 основных нитей ленты, со сдвигом рядов в соседних слоях на (0,4-0,6)l, где l - расстояние между рядами - признаки соответствуют критерию «изобретательский уровень», предусматривают новое взаимное расположение элементов и новое соотношение размеров, направлены на решение поставленной задачи с достижением технического результата, на повышение надежности работы чехла за счет оптимального распределения напряжений в соединениях волокон слоев многослойного чехла, работающего как рулонно-тканные емкости давления, имеющие картину разрушения «размотом» ткани;- adhesive points are arranged in rows in a checkerboard pattern with a distance between the rows equal to the distance between the points in the rows, which is determined based on the arrangement between the points 40-120 of the main threads of the tape, with the rows shifted in adjacent layers by (0.4-0.6 ) l, where l is the distance between the rows - the signs meet the criterion of "inventive step", provide for a new mutual arrangement of elements and a new size ratio, aimed at solving the problem with achieving a technical result, to increase reliability the work of the cover due to the optimal distribution of stresses in the fiber connections of the layers of the multilayer cover working as rolled-woven pressure vessels having a pattern of destruction by "unwinding" of the fabric;

- клеевые точки выполнены с уменьшением расстояния между точками в процессе намотки от lн до lк=(0,4-0,8)lн, где:- adhesive points are made with decreasing the distance between the points during the winding process from l n to l k = (0.4-0.8) l n , where:

- lн - расстояние между точками в начале намотки на первом слое;- l n - the distance between the points at the beginning of the winding on the first layer;

- lк - расстояние между точками в конце намотки на последнем слое - признаки соответствуют критерию «изобретательский уровень», предусматривают новое взаимное расположение элементов и новое соотношение размеров, направлены на решение поставленной задачи с достижением технического результата, на повышение надежности работы чехла за счет оптимального распределения сдвиговых напряжений в соединениях волокон слоев многослойного чехла, работающего как рулонно-тканные емкости давления, с увеличением сдвиговых усилий от внутреннего слоя к наружному, имеющие картину разрушения «размотом» ткани, начиная от наружной кромки;- l to - the distance between the points at the end of the winding on the last layer - the signs meet the criterion of "inventive step", provide for a new mutual arrangement of elements and a new size ratio, aimed at solving the problem with achieving a technical result, to improve the reliability of the cover due to the optimal the distribution of shear stresses in the fiber joints of the layers of a multilayer sheath that acts as a roll-woven pressure vessel, with an increase in shear forces from the inner layer to external, having a picture of destruction by "unwinding" of the fabric, starting from the outer edge;

- камера выполнена из армированного материала объемом, превышающим внутренний объем чехла на 0,4-2,4% - признаки соответствуют критерию «изобретательский уровень», предусматривают обоснованное применение новых материалов и новое соотношение размеров, направлены на решение поставленной задачи с достижением технического результата, на повышение надежности работы (что подтверждено исследованиями) и снижение массы изделия;- the camera is made of reinforced material with a volume exceeding the internal volume of the cover by 0.4-2.4% - the signs meet the criterion of "inventive step", provide for the justified use of new materials and a new size ratio, aimed at solving the problem with achieving a technical result, to increase the reliability of work (as confirmed by research) and reduce the mass of the product;

- домкрат-подушка размещена в защитной прорезиненной оболочке, снабженной снаружи протекторами - признаки соответствуют критерию «изобретательский уровень», предусматривают наличие новых элементов и их новое взаимное расположение, направлены на решение поставленной задачи с достижением технического результата, на повышение надежности работы домкрата-подушки за счет его защиты от внешних воздействий при хранении, а также за счет повышения коэффициента трения рабочих поверхностей.- the cushion jack is placed in a rubberized protective shell provided with protectors on the outside - the signs meet the criterion of “inventive step”, provide for the presence of new elements and their new relative position, are aimed at solving the problem with achieving a technical result, to increase the reliability of the cushion jack for due to its protection against external influences during storage, as well as by increasing the coefficient of friction of the working surfaces.

Указанные отличительные признаки являются существенными, поскольку каждый в отдельности и все совместно направлены на решение поставленной задачи с достижением технических результатов. Использование единой совокупности существенных отличительных признаков в известных решениях не обнаружено, что характеризует соответствие технического решения критерию «новизна».These distinguishing features are significant, since each individually and all together are aimed at solving the problem with the achievement of technical results. The use of a single set of essential distinguishing features in the known solutions was not found, which characterizes the conformity of the technical solution to the criterion of "novelty."

Единая совокупность новых существенных признаков с общими известными обеспечивает решение поставленной задачи с достижением технических результатов и характеризует предложенные технические решения существенными отличиями по сравнению с известным уровнем техники и аналогами. Данные технические решения являются результатом научно-исследовательской и экспериментальной работы по повышению технологичности конструкции домкрата-подушки и повышению надежности ее работы без использования известных проектировочных решений, рекомендаций, материалов и обладают неочевидностью, что свидетельствует об их соответствии критерию «изобретательский уровень».A single set of new essential features with common known provides a solution to the problem with the achievement of technical results and characterizes the proposed technical solutions by significant differences compared with the prior art and analogues. These technical solutions are the result of research and experimental work to increase the manufacturability of the design of the jack-pillow and increase the reliability of its operation without the use of well-known design solutions, recommendations, materials and are non-obvious, which indicates their compliance with the criterion of "inventive step".

Сущность изобретений поясняется чертежами, где на фиг.1 представлен общий вид домкрата-подушки, на фиг.2 - общий вид способа изготовления домкрата-подушки, на фиг.3 - способ намотки чехла, на фиг.4 - сечение угла домкрата-подушки, на фиг.5 - сечение угла со штуцером, на фиг.6 - поперечное сечение штуцера в зоне его крепления, на фиг.7 - сечение нагруженного внутренним давлением домкрата-подушки, на фиг.8 - сечение домкрата-подушки, нагруженного внутренним давлением и внешним воздействием.The invention is illustrated by drawings, where figure 1 shows a General view of the jack-pillow, figure 2 is a General view of the manufacturing method of the jack-pillow, figure 3 is a method of winding a cover, figure 4 is a cross section of the corner of the jack-pillow, figure 5 is a cross section of the angle with the fitting, figure 6 is a cross section of the fitting in the area of its attachment, figure 7 is a section of a jack-cushion loaded with internal pressure, figure 8 is a section of a jack-cushion loaded with internal pressure and external exposure.

Способ изготовления домкрата-подушки 1, при котором на герметичную камеру 2 в форме равностороннего треугольника из тонкостенного упруго-эластичного материала со штуцером 3 в ее углу наматывают чехол 4 из 5-15 слоев 5 непрерывной ленты 6 из высокопрочной ткани шириной, соответствующей высоте треугольника камеры, выполняя линии 7 сгиба 8 ленты 6 под углом 60° к продольным краям 9 ленты 5, обертывая этими краями 9 штуцер 3, скрепляя соседние слои 5 преимущественно в площади вписанного в треугольник круга 10 точечными клеевыми упруго-эластичными соединениями 11 с дополнительным скреплением 12 слоев 5 в углах треугольного чехла.A method of manufacturing a cushion jack 1, in which a cover 4 of 5-15 layers 5 of a continuous tape 6 of high strength fabric with a width corresponding to the height of the triangle of the chamber is wound on a sealed chamber 2 in the form of an equilateral triangle of thin-walled elastic material with a fitting 3 in its corner , fulfilling the lines 7 of the bend 8 of the tape 6 at an angle of 60 ° to the longitudinal edges 9 of the tape 5, wrapping the nozzles 3 with these edges 9, fastening the adjacent layers 5 mainly in the area of the circle 10 inscribed in the triangle by point adhesive elastic compounds eniyami 11 to 12 additional bonding layers 5 in the corners of the triangular bag.

Углы камеры притупляют радиусом или фаской 13.The corners of the camera dull with a radius or chamfer 13.

Скрепление 14 слоев 5 в углах чехла 4 выполняют их пропиткой 15 упруго-эластичной композицией.Bonding 14 layers 5 in the corners of the cover 4 is performed by impregnating them 15 with an elastic-elastic composition.

Скрепление 14 слоев 5 в углах без штуцера 3 выполняют сквозной прошивкой 16 без повреждения камеры 2.Bonding 14 layers 5 in the corners without fitting 3 is performed through firmware 16 without damaging the camera 2.

Скрепление слоев 5 и штуцера 3 выполняют обмоткой 17 пропитанным упруго-эластичной композицией жгутом 19 или пропитанной нитью.The fastening of the layers 5 and the fitting 3 is carried out by winding 17 with a bundle 19 impregnated with an elastic-elastic composition or an impregnated thread.

Клеевые точки 11 располагают рядами в шахматном порядке с расстоянием между рядами, равным расстоянию между точками в рядах, которое определяют исходя из условия расположения между точками 40-120 основных нитей 20 ленты со сдвигом рядов в соседних слоях на (0,4-0,6)l, где l - расстояние между рядами.The glue points 11 are arranged in rows in a checkerboard pattern with the distance between the rows equal to the distance between the points in the rows, which is determined based on the arrangement between the points 40-120 of the main threads 20 of the tape with the rows shifted in adjacent layers by (0.4-0.6 ) l, where l is the distance between the rows.

Клеевые точки 11 выполняют с уменьшением расстояния между точками в процессе намотки от lн до lк=(0,4-0,8)lн, где:The glue points 11 are performed with decreasing the distance between the points during the winding process from l n to l k = (0.4-0.8) l n , where:

- lн - расстояние между точками в начале намотки на первом слое;- l n - the distance between the points at the beginning of the winding on the first layer;

- lк - расстояние между точками в конце намотки на последнем слое.- l to - the distance between the points at the end of the winding on the last layer.

Камеру 2 выполняют из армированного материала объемом, превышающим внутренний объем чехла на 0,4-2,4%.Chamber 2 is made of reinforced material with a volume exceeding the internal volume of the cover by 0.4-2.4%.

Домкрат-подушку 1 размещают в защитной прорезиненной оболочке 21, снабженной снаружи протекторами 22.The cushion jack 1 is placed in a protective rubberized shell 21 provided with protectors 22 on the outside.

Домкрат-подушка 1, включающая герметичную 2 камеру в форме равностороннего треугольника из тонкостенного упруго-эластичного материала со штуцером 3 в ее углу, чехол 4 из 5-15 слоев 5 непрерывной ленты 6 из высокопрочной ткани шириной, соответствующей высоте треугольника камеры 2, намотанный на камеру 2 сгибанием 8 ленты 6 под углом 60° к продольным краям 9 ленты 6 с обертыванием этими краями 9 штуцера 3, причем соседние слои 5 скреплены преимущественно в площади вписанного в треугольник круга 10 точечными клеевыми упруго-эластичными соединениями 11 с дополнительным скреплением 12 слоев 5 в углах треугольного чехла.A cushion jack 1, including a sealed chamber 2 in the form of an equilateral triangle of thin-walled elastic material with a fitting 3 in its corner, a cover 4 of 5-15 layers 5 of a continuous tape 6 made of high-strength fabric with a width corresponding to the height of the triangle of the chamber 2, wound around the chamber 2 by bending 8 of the tape 6 at an angle of 60 ° to the longitudinal edges 9 of the tape 6 with wrapping these edges 9 of the fitting 3, and the adjacent layers 5 are bonded mainly in the area of the circle 10 inscribed in the triangle by point adhesive elastic-elastic joints 11 s additional fastening of 12 layers 5 in the corners of a triangular cover.

Углы камеры притуплены радиусом или фаской 13.The corners of the chamber are blunted with a radius or chamfer 13.

Слои 5 в углах чехла 4 скреплены упруго-эластичной композицией 15.Layers 5 in the corners of the cover 4 are bonded with an elastic-elastic composition 15.

Слои 5 в углах без штуцера 3 скреплены сквозной прошивкой 16 без повреждения камеры 2.Layers 5 in the corners without fitting 3 are fastened with through firmware 16 without damaging the camera 2.

Слои 5 и штуцер 3 скреплены обмоткой пропитанным упруго-эластичной композицией жгутом 19 или пропитанной нитью.Layers 5 and nozzle 3 are fastened together by a winding with a strand 19 impregnated with an elastic-elastic composition or an impregnated thread.

Клеевые точки 11 расположены рядами в шахматном порядке с расстоянием между рядами, равным расстоянию между точками в рядах, которое определено исходя из условия расположения между точками 40-120 основных нитей 20 ленты 6 со сдвигом рядов в соседних слоях на (0,4-0,6)l, где l - расстояние между рядами.The glue points 11 are arranged in rows in a staggered manner with a distance between the rows equal to the distance between the points in the rows, which is determined based on the arrangement between the points 40-120 of the main threads 20 of the tape 6 with the rows shifted in adjacent layers by (0.4-0, 6) l, where l is the distance between the rows.

Клеевые точки 11 выполнены с уменьшением расстояния между точками в процессе намотки от lн до lк=(0,4-0,8)lн, где:The glue points 11 are made with decreasing the distance between the points during winding from l n to l k = (0.4-0.8) l n , where:

- lн - расстояние между точками в начале намотки на первом слое;- l n - the distance between the points at the beginning of the winding on the first layer;

- lк - расстояние между точками в конце намотки на последнем слое.- l to - the distance between the points at the end of the winding on the last layer.

Камера 2 выполнена из армированного материала объемом, превышающим внутренний объем чехла на 0,4-2,4%.The chamber 2 is made of reinforced material with a volume exceeding the internal volume of the cover by 0.4-2.4%.

Домкрат-подушка 1 размещена в защитной прорезиненной оболочке 21, снабженной снаружи протекторами 22.The cushion jack 1 is housed in a protective rubberized shell 21 provided with protectors 22 on the outside.

Пример конкретного исполнения способа заключается в том, что на герметичную камеру 2 в форме равностороннего треугольника из тонкостенного упруго-эластичного материала со штуцером 3 в ее углу наматывают со ступенчатым изменением на 60° направления намотки чехол 4 из 5-15 слоев 5 ленты 6 из высокопрочной ткани шириной, соответствующей высоте треугольника камеры 2 с учетом припуска ленты 6 на скрепление слоев 5 в углах. Скрепление слоев 5 и штуцера 3 выполняют обмоткой 17 с натяжением 18 пропитанным упруго-эластичной композицией жгутом 19 или пропитанной нитью.An example of a specific embodiment of the method is that on a sealed chamber 2 in the form of an equilateral triangle of thin-walled elastic material with a fitting 3 in its corner, a cover 4 of 5-15 layers 5 of tape 6 of high strength is wound with a step change of 60 ° fabric width corresponding to the height of the triangle of the chamber 2, taking into account the allowance of the tape 6 for bonding layers 5 in the corners. The fastening of the layers 5 and the fitting 3 is performed by a winding 17 with a tension of 18, a bundle 19 impregnated with an elastic-elastic composition, or a thread impregnated.

Пример конкретного исполнения домкрата-подушки 1 заключается в том, что для клеевых соединений 11, пропиток 15 слоев 5 в углах и пропитки жгута 19 обмотки 17 штуцера 3 использован эластичный клей на основе полиуретана, что улучшает условия хранения (гибкость при складывании), а также удобство применения в ограниченном пространстве. Все силовые соединения (текстильные швы 16, клеевые соединения 15 и обмотка 17) выполнены на участках с минимальными радиусами кривизны, где по условиям работы рулонно-тканной емкости давления действуют минимальные напряжения (нормальные - в волокнах тканей и сдвиговые межслоевые). Выполнены эти соединения в углах чехла. С учетом картины разрушения рулонно-тканной емкости давления - «размотом», начиная от наружной кромки наружного слоя, клеевые соединения 11 выполнены с возрастающей интенсивностью - от внутренней кромки внутреннего слоя к наружной кромке наружного слоя, которая пропитана клеем и приклеена по всей длине, что также препятствует разрушению самой кромки от разлохмачивания волокон ткани.An example of a specific implementation of the cushion jack 1 is that for adhesive joints 11, impregnation of 15 layers 5 in the corners and impregnation of the tow band 19 of the winding 17 of the fitting 3, an elastic adhesive based on polyurethane is used, which improves storage conditions (folding flexibility), and ease of use in confined spaces. All power joints (textile seams 16, adhesive joints 15 and winding 17) are made in areas with minimal radii of curvature, where, under the conditions of the roll-woven fabric pressure tank, the minimum stresses (normal in the fabric fibers and shear interlayer). These connections are made in the corners of the cover. Given the pattern of destruction of the roll-woven pressure vessel - “unwinding”, starting from the outer edge of the outer layer, adhesive joints 11 are made with increasing intensity - from the inner edge of the inner layer to the outer edge of the outer layer, which is impregnated with glue and glued along the entire length, which also prevents the destruction of the edge itself from razlohmachivaemosti tissue fibers.

Работает домкрат-подушка 1 следующим образом. При нагружении оболочки из чехла 4 внутренним давлением 23 без внешних воздействий (см. фиг.7) она принимает в поперечном сечении каплевидную форму. При внешнем воздействии 24 оболочка деформируется (см. фиг.8), обеспечивая грузоподъемность, равную произведению давления 23 на площадь пятна контакта. Увеличение высоты подъема 25 достигается повышением давления 23.The jack-pillow 1 works as follows. When loading the shell from the cover 4 with internal pressure 23 without external influences (see Fig. 7), it takes a drop-shaped cross section. Under external influence 24, the shell is deformed (see Fig. 8), providing a load capacity equal to the product of pressure 23 by the area of the contact spot. The increase in lifting height 25 is achieved by increasing the pressure 23.

Таким образом, использование изобретения позволит создать высокотехнологичную конструкцию домкрата-подушки с повышенной надежностью работы, что и подтверждает использование изобретения по назначению. Осуществимость изобретений подтверждена положительными результатами испытаний образцов домкратов-подушек, разработка и изготовление которых полностью основаны на представленном описании. В связи с этим новое техническое решение соответствует критерию «промышленная применимость», т.е. уровню изобретения.Thus, the use of the invention will allow to create a high-tech design of the jack-pillow with increased reliability, which confirms the use of the invention for its intended purpose. The feasibility of the invention is confirmed by the positive test results of samples of jacks-pillows, the development and manufacture of which are completely based on the description. In this regard, the new technical solution meets the criterion of "industrial applicability", ie level of invention.

Claims (18)

1. Способ изготовления домкрата-подушки, при котором на герметичную камеру в форме равностороннего треугольника из тонкостенного упругоэластичного материала со штуцером в ее углу наматывают чехол из 5-15 слоев непрерывной ленты из высокопрочной ткани шириной, соответствующей высоте треугольника камеры, выполняя линии сгиба ленты под углом 60° к продольным краям ленты, обертывая этими краями штуцер, скрепляя соседние слои преимущественно в площади вписанного в треугольник круга точечными клеевыми упругоэластичными соединениями, с дополнительным скреплением слоев в углах треугольного чехла.1. A method of manufacturing a cushion jack, in which a cover of 5-15 layers of a continuous tape of high-strength fabric with a width corresponding to the height of the triangle of the chamber is wound on a sealed chamber in the shape of an equilateral triangle of thin-walled elastic material with a fitting in its corner, making tape bend lines under at an angle of 60 ° to the longitudinal edges of the tape, wrapping the fitting around these edges, fastening the adjacent layers mainly in the area of the circle inscribed in the triangle by point adhesive elastic compounds, with additional by stitching layers in the corners of a triangular cover. 2. Способ по п.1, отличающийся тем, что углы камеры притупляют радиусом или фаской.2. The method according to claim 1, characterized in that the corners of the camera dull the radius or bevel. 3. Способ по п.1, отличающийся тем, что скрепление слоев в углах чехла выполняют их пропиткой упругоэластичной композицией.3. The method according to claim 1, characterized in that the bonding of the layers in the corners of the cover perform their impregnation with an elastic composition. 4. Способ по п.1, отличающийся тем, что скрепление слоев в углах без штуцера выполняют сквозной прошивкой без повреждения камеры.4. The method according to claim 1, characterized in that the bonding of the layers in the corners without a fitting is performed through firmware without damaging the camera. 5. Способ по п.1, отличающийся тем, что скрепление слоев и штуцера выполняют обмоткой пропитанным упругоэластичной композицией жгутом или пропитанной нитью.5. The method according to claim 1, characterized in that the bonding of the layers and the fitting is carried out by winding a bundle impregnated with an elastic composition, or with an impregnated thread. 6. Способ по п.1, отличающийся тем, что клеевые точки располагают рядами в шахматном порядке с расстоянием между рядами, равным расстоянию между точками в рядах, которое определяют, исходя из условия расположения между точками 40-120 основных нитей ленты, со сдвигом рядов в соседних слоях на (0,4-0,6)l, где l - расстояние между рядами.6. The method according to claim 1, characterized in that the adhesive points are arranged in rows staggered with a distance between the rows equal to the distance between the points in the rows, which is determined based on the arrangement between the points 40-120 of the main threads of the tape, with the rows shifted in adjacent layers by (0.4-0.6) l, where l is the distance between the rows. 7. Способ, по п.6, отличающийся тем, что клеевые точки выполняют с уменьшением расстояния между точками в процессе намотки от lн до lк=(0,4-0,8)lн,
где lн - расстояние между точками в начале намотки на первом слое;
lк - расстояние между точками в конце намотки на последнем слое.
7. The method according to claim 6, characterized in that the adhesive points are performed with decreasing the distance between the points during winding from l n to l k = (0.4-0.8) l n ,
where l n - the distance between the points at the beginning of the winding on the first layer;
l to - the distance between the points at the end of the winding on the last layer.
8. Способ по п.1, отличающийся тем, что камеру выполняют из армированного материала объемом, превышающим внутренний объем чехла на 0,4-2,4%.8. The method according to claim 1, characterized in that the chamber is made of reinforced material with a volume exceeding the internal volume of the cover by 0.4-2.4%. 9. Способ по п.1, отличающийся тем, что домкрат-подушку размещают в защитной прорезиненной оболочке, снабженной снаружи протекторами.9. The method according to claim 1, characterized in that the jack-pillow is placed in a protective rubberized shell provided with protectors on the outside. 10. Домкрат-подушка, включающая герметичную камеру в форме равностороннего треугольника из тонкостенного упругоэластичного материала со штуцером в ее углу, чехол из 5-15 слоев непрерывной ленты из высокопрочной ткани шириной, соответствующей высоте треугольника камеры, намотанный на камеру сгибанием ленты под углом 60° к продольным краям ленты, с обертыванием этими краями штуцера, причем соседние слои скреплены преимущественно в площади вписанного в треугольник круга точечными клеевыми упругоэластичными соединениями, с дополнительным скреплением слоев в углах треугольного чехла.10. A cushion jack, including a sealed chamber in the form of an equilateral triangle of thin-walled elastic material with a fitting in its corner, a cover of 5-15 layers of continuous tape of high-strength fabric with a width corresponding to the height of the chamber triangle, wound around the camera by bending the tape at an angle of 60 ° to the longitudinal edges of the tape, with a fitting wrapped around these edges, the adjacent layers being bonded predominantly in the area of the circle inscribed in the triangle by point adhesive elastic joints with additional repleniem layers in the corners of the triangular cover. 11. Домкрат-подушка по п.10, отличающаяся тем, что углы камеры притуплены радиусом или фаской.11. The cushion jack of claim 10, wherein the corners of the chamber are blunted with a radius or chamfer. 12. Домкрат-подушка по п.10, отличающаяся тем, что слои в углах чехла скреплены упругоэластичной композицией.12. The cushion jack of claim 10, characterized in that the layers in the corners of the cover are fastened with an elastic composition. 13. Домкрат-подушка по п.10, отличающаяся тем, что слои в углах без штуцера скреплены сквозной прошивкой без повреждения камеры.13. The jack-pad according to claim 10, characterized in that the layers in the corners without a fitting are fastened with through firmware without damaging the camera. 14. Домкрат-подушка по п.10, отличающаяся тем, что слои и штуцер скреплены обмоткой пропитанным упругоэластичной композицией жгутом или пропитанной нитью.14. A cushion jack according to claim 10, characterized in that the layers and the fitting are fastened together by a winding with a tourniquet impregnated with an elastic composition, or with an impregnated thread. 15. Домкрат-подушка по п.10, отличающаяся тем, что клеевые точки расположены рядами в шахматном порядке с расстоянием между рядами, равным расстоянию между точками в рядах, которое определено, исходя из условия расположения между точками 40-120 основных нитей ленты, со сдвигом рядов в соседних слоях на (0,4-0,6)l, где l - расстояние между рядами.15. The cushion jack of claim 10, wherein the adhesive points are arranged in rows in a checkerboard pattern with a distance between rows equal to the distance between the points in the rows, which is determined based on the arrangement between the points 40-120 of the main threads of the tape, with by shifting the rows in adjacent layers by (0.4-0.6) l, where l is the distance between the rows. 16. Домкрат-подушка по п.15, отличающаяся тем, что клеевые точки выполнены с уменьшением расстояния между точками в процессе намотки от lн до lк=(0,4-0,8)lн,
где lн - расстояние между точками в начале намотки на первом слое;
lк - расстояние между точками в конце намотки на последнем слое.
16. The cushion jack according to claim 15, wherein the adhesive points are made with decreasing the distance between the points during winding from l n to l k = (0.4-0.8) l n ,
where l n - the distance between the points at the beginning of the winding on the first layer;
l to - the distance between the points at the end of the winding on the last layer.
17. Домкрат-подушка по п.10, отличающаяся тем, что камера выполнена из армированного материала объемом, превышающим внутренний объем чехла на 0,4-2,4%.17. The cushion jack of claim 10, wherein the chamber is made of reinforced material with a volume exceeding the internal volume of the cover by 0.4-2.4%. 18. Домкрат-подушка по п.10, отличающаяся тем, что она размещена в защитной прорезиненной оболочке, снабженной снаружи протекторами. 18. The cushion jack of claim 10, characterized in that it is placed in a protective rubberized shell provided with protectors on the outside.
RU2010151651/11A 2010-12-15 2010-12-15 Method of fabricating jack-pad and said jack-pad RU2453492C1 (en)