KR20190121268A - Method of manufacturing recycled aggregate and normal temperature ascon manufactured by using the same - Google Patents

Method of manufacturing recycled aggregate and normal temperature ascon manufactured by using the same Download PDF

Info

Publication number
KR20190121268A
KR20190121268A KR1020190074044A KR20190074044A KR20190121268A KR 20190121268 A KR20190121268 A KR 20190121268A KR 1020190074044 A KR1020190074044 A KR 1020190074044A KR 20190074044 A KR20190074044 A KR 20190074044A KR 20190121268 A KR20190121268 A KR 20190121268A
Authority
KR
South Korea
Prior art keywords
ascon
recycled aggregate
room temperature
aggregate
crushed
Prior art date
Application number
KR1020190074044A
Other languages
Korean (ko)
Other versions
KR102213683B1 (en
Inventor
신시종
Original Assignee
주식회사 다현산업
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 주식회사 다현산업 filed Critical 주식회사 다현산업
Priority to KR1020190074044A priority Critical patent/KR102213683B1/en
Publication of KR20190121268A publication Critical patent/KR20190121268A/en
Application granted granted Critical
Publication of KR102213683B1 publication Critical patent/KR102213683B1/en

Abstract

The present invention relates to a manufacturing method of a recycled aggregate for room temperature ascon, which comprises the steps of: preparing a product to be crushed for the recycled aggregate by crushing concrete waste and performing size selection; washing the product to be crushed; and sequentially stacking in the product to be crushed of a washed wet state on a conveyor belt equipped with a plurality of far-infrared heaters, and drying and conveying the same. Because the moisture content of the recycled aggregate dried by the method can be adjusted, physical properties compared to ascon using new aggregates are further improved, while lowering the unit cost of the ascon manufactured using the same.

Description

재생 골재의 제조방법 및 이를 이용하여 제조된 상온 아스콘{METHOD OF MANUFACTURING RECYCLED AGGREGATE AND NORMAL TEMPERATURE ASCON MANUFACTURED BY USING THE SAME} Manufacturing method of recycled aggregate and room temperature ascone manufactured using the same {METHOD OF MANUFACTURING RECYCLED AGGREGATE AND NORMAL TEMPERATURE ASCON MANUFACTURED BY USING THE SAME}

본 기술은 아스콘 제조 분야의 기술로서, 보다 상세하게는 폐골재 파쇄물의 건조를 위하여 신규 방식을 채용함으로써 재생골재를 용이하게 제조할 수 있고, 나아가 재생골재를 사용함에도 신규 골재를 이용하여 제조된 아스콘보다도 더욱 우수한 물성을 갖는 아스콘을 제조할 수 있는 기술에 관한 것이다. The present technology is a technology in the field of ascon production, and more specifically, it is possible to easily produce recycled aggregates by adopting a new method for drying waste aggregate crushed products. The present invention relates to a technology capable of producing ascon having more excellent physical properties.

종래의 도로보수 방법은 역청 혼합물을 KS F 2349 공법에 따라서 가열혼합 및 가열포설 하는 공정인데, 상기 혼합물은 쇄석 및 자갈, 잔골재 등을 170∼180 ℃ 고온으로 가열 및 건조한 다음 이 건조물에 140∼150 ℃로 가열한 스트레이트 아스팔트를 결합재로서 적정량 가하고 이들을 고온에서 혼합한 고온 아스콘으로 제조된다. 그러나 이러한 방법으로 제조된 고온 아스콘은 아스팔트 특성상 온도가 내려가면 결합재의 점성이 급격히 증대하여 덩어리로 되므로, 이를 방지하기 위해서는 상기 역청 혼합물을 130∼140 ℃로 유지하면서 제한 시간 내에 포장해야만 하는 불편이 야기되었으며, 또한 장거리 수송이 어려울 뿐만 아니라 겨울철 공사시에는 재료분리가 일어날 우려가 있다. 특히, 도로 파손이 소규모일 경우에는 대단위의 아스콘을 사용하기가 곤란하다는 문제가 있다. 상기 언급한 바와 같은 고온 아스콘(가열식 아스콘이라고도 한다)을 도로 보수용으로 사용할 때 발생하는 여러 가지 문제점을 해결하기 위해 상온 혼합 및 상온 포설이 가능한 상온 아스콘이 제안되었다.The conventional road repairing method is a process of mixing and heating the bitumen mixture according to the KS F 2349 method, and the mixture is heated and dried at a high temperature of 170 to 180 ° C. with crushed stone, gravel and fine aggregates and then to 140 to 150 in this dry matter. An appropriate amount of straight asphalt heated to 0 ° C. is added as a binder and a high temperature ascon mixed with these at high temperature. However, the high temperature ascon prepared by this method is rapidly increased in viscosity due to the characteristics of the asphalt, the viscosity of the binder becomes agglomerate, and in order to prevent this, it is inconvenient to maintain the bitumen mixture at 130-140 ° C. and to pack it within a limited time. It is also difficult to transport long distances, and there is a risk of material separation during winter construction. In particular, there is a problem that it is difficult to use a large unit of asphalt when the road damage is small. In order to solve various problems that occur when the high temperature ascon (also referred to as a heated ascon) for road repair as mentioned above, a room temperature ascon which is capable of mixing at room temperature and laying at room temperature has been proposed.

아스콘(Ascon)은 아스팔트 콘크리트(Asphalt Concrete)를 줄인 명칭이며, 일반적으로 아스팔트(asphalt)와 굵은 골재(자갈:Aggregate), 잔골재(모래:Sand) 또는 포장용 채움재(필러,석분:mineral filler)를 가열하거나 상온으로 혼합한 것으로 도로포장이나 주차장 등에 주로 사용되고 있으며, 사용목적 이나 용도, 기능, 공법에 따라 여러 가지로 구분하고 있다.Ascon is shortened asphalt concrete and is generally used to heat asphalt and coarse aggregate (gravel), fine aggregate (sand) or pavement material (filler, mineral filler). They are mixed at room temperature and are mainly used for road pavement or parking lot, and are classified into various types according to the purpose of use, use, function, and construction method.

한편, 상온 아스콘에 사용되는 골재로 재생골재가 사용되기도 한다. 재생 골재를 제조하기 위해서는 폐골재를 세척하고 건조하는 단계를 거쳐야 한다. 상기 건조를 위해서 종래에는 드럼방식의 건조 방법이 사용되 오고 있다. 이 방식은 대형 드럼 건조기 내에 세척된 폐골재를 넣고 일괄적으로 건조하는 방식이다. 그러나 이러한 드럼방식의 건조는 설비비가 매우 크고 넓은 설치 장소를 요구한다. 또한, 이 방식은 대량의 폐골재에 대하여 크기 분리를 진행해야 하므로 재료 분리를 위한 부담이 큰 방식이다.On the other hand, recycled aggregates are also used as aggregates used in room temperature ascon. In order to produce recycled aggregates, the waste aggregates must be washed and dried. Conventionally, a drum drying method has been used for the drying. This method puts the waste aggregate washed in a large drum dryer and batch drying. However, such drum drying requires a large installation cost and a large installation cost. In addition, this method is a heavy burden for the material separation because the size separation must proceed for a large amount of waste aggregate.

나아가 드럼 방식의 건조 방법은 폐골재에 대한 건조 정도를 조절하기 어렵고, 균일한 건조가 어려운 문제점이 있다. Furthermore, the drum method has a problem in that it is difficult to control the degree of drying of the waste aggregate, and uniform drying is difficult.

본 발명은 이러한 종래의 드럼 방식의 건조 공정이 갖는 문제점을 극복하고자 도출된 발명으로서, 폐골재의 크기 분리가 용이하고 작업자의 의도에 따라 건조 정도를 용이하게 조절할 수 있으며 건조 중 발생할 수 있는 분진 날림을 방지할 수 있는 상온 아스콘용 재생 골재의 제조방법을 제공하는 것을 목적으로 한다.The present invention is derived to overcome the problems of the conventional drum-type drying process, it is easy to separate the size of the waste aggregate, can easily control the degree of drying according to the intention of the operator and dust blowing that can occur during drying An object of the present invention is to provide a method for producing a recycled aggregate for room temperature ascone can be prevented.

또한, 본 발명은 상기와 같이 제조된 재생골재를 포함함에도 신규 골재를 이용한 아스콘 대비 오히려 물성이 더욱 향상된 상온 아스콘을 제공하는 것을 목적으로 한다. In addition, an object of the present invention is to provide a room temperature ascon more improved physical properties compared to ascon using new aggregates, including the recycled aggregate prepared as described above.

본 발명의 일 실시예에 따른 상온 아스콘용 재생골재의 제조방법은 콘크리트 폐기물을 파쇄하고 크기를 선별하여 재생골재용 파쇄물을 준비하는 단계; 상기 파쇄물을 세척하는 단계; 및 세척된 젖은 상태의 파쇄물을 복수의 원적외선 히터가 구비된 컨베이어 벨트에 순차적으로 적재하여 이송하면서 건조시키는 단계를 포함한다. Method for producing a recycled aggregate for room temperature asphalt concrete according to an embodiment of the present invention comprises the steps of preparing a crushed aggregate for crushing the concrete waste and screening the size; Washing the debris; And drying the washed wet debris while being sequentially loaded and transported on a conveyor belt equipped with a plurality of far infrared heaters.

상기 파쇄물은 8mm 이하의 크기로 선별되는 것이 바람직하다.The crushed material is preferably selected to a size of 8mm or less.

상기 적재된 파쇄물은 컨페이어 벨트 상에 배치된 로터리 형태의 서로 다른 크기를 갖는 복수의 혼합기에 의하여 혼합됨으로써 균일하게 건조될 수 있다.The loaded debris can be uniformly dried by mixing by means of a plurality of mixers of different sizes in the form of rotarys disposed on the conveyor belt.

상기 컨베이어 벨트 상에는 열반사기 및 온도 센서가 구비되어 있다.A heat reflector and a temperature sensor are provided on the conveyor belt.

상기 건조는 상기 원적외선 히터의 발열량을 조절함으로써 재생골재의 온도가 40 내지 50℃의 온도가 되도록 한다. 한편, 상기 건조는 건조된 재생골재에 수분이 잔존하도록 이루어진다.The drying is such that the temperature of the recycled aggregate is a temperature of 40 to 50 ℃ by adjusting the calorific value of the far infrared heater. On the other hand, the drying is made so that moisture remains in the dried recycled aggregate.

상기 원적외선 히터는 LPG 가스 또는 전기를 이용하여 발열되는 히터이다.The far infrared heater is a heater that generates heat using LPG gas or electricity.

본 발명의 일 실시예에 따른 상온 아스콘은 전술한 방식으로 제조된 8mm 이하의 크기를 갖는 재생골재 50 내지 90 중량%; 4 내지 8mm의 크기를 갖는 신골재 10 내지 50 중량%; 결합재로서 비가열 아스팔트 4 내지 10 중량%; 및 박리 방지제로서 다이머산 0.04 내지 1.5 중량%를 포함한다. Room temperature ascon according to an embodiment of the present invention 50 to 90% by weight recycled aggregate having a size of 8mm or less prepared in the above-described manner; 10 to 50% by weight of new aggregate having a size of 4 to 8mm; 4 to 10% by weight of unheated asphalt as a binder; And 0.04 to 1.5% by weight of dimer acid as the anti-peeling agent.

본 발명에 따른 재생골재의 제조방법은 폐콘크리트 파쇄물을 이용하기 때문에, 골재 성분 외에 폐콘크리트에 혼합되어 있는 각종 채움재 등의 기능성 성분까지 재활용될 수 있다. 따라서 본 방법은 아스콘 혼합 과정에 사용되는 혼합성분 중 다수의 혼합요소를 배제할 수 있어, 재생골재를 이용한 제조 단가 감소뿐만 아니라 아스콘 혼합 과정에서도 사용되는 재료의 절약이 가능하여 매우 경제적이다.Since the method for producing recycled aggregate according to the present invention uses waste concrete crushed material, it can be recycled to functional components such as various fillers mixed with waste concrete in addition to the aggregate component. Therefore, the present method can exclude a large number of mixing elements among the mixed components used in the ascon mixing process, it is possible to save the material used in the ascon mixing process as well as to reduce the manufacturing cost using recycled aggregate is very economical.

또한, 상기 재생골재의 제조방법은 세척되어 젖어있는 폐콘크리트 파쇄물을 건조하기 위한 방법으로서, 기존의 드럼 방식이 아닌 원적외선히터가 구비된 컨베이어 벨트를 이용하여 건조하는 방법을 도입하고 있어 연속적인 건조가 가능하고 크기 선별 등 재료 분리가 용이하다. 상기 원적외선 히터는 LPG 가스를 이용하여 구동되기 때문에 바람이 발생하지 않아 건조 과정 중에 발생할 수 있는 분진 날림 등이 방지될 수 있다. 본 실시예에서는 원적외선히터가 LPG 가스를 발열원으로 사용하는 것으로 기재하였으나, 이와 다르게 전기를 이용한 원적외선 히터를 사용하여도 무방하다.In addition, the manufacturing method of the recycled aggregate is a method for drying the washed and wet concrete crushed material, it is introduced by a method of drying using a conveyor belt equipped with a far-infrared heater instead of the conventional drum method, continuous drying It is possible to separate materials such as size selection. Since the far-infrared heater is driven using LPG gas, no wind is generated and dust blowing, which may occur during the drying process, may be prevented. In the present embodiment, the far-infrared heater is described as using LPG gas as a heat generating source. Alternatively, the far-infrared heater using electricity may be used.

한편, 상기 컨베이어 벨트 상에는 로터리 형태의 소형 및 대형 혼합기가 연속적으로 배치되어 건조되는 폐골재 파쇄물을 지속적으로 고르게 펴거나 굴려 줄 수 있기 때문에 파쇄물의 균일한 건조가 가능하다.On the other hand, on the conveyor belt it is possible to uniformly dry or crush the waste aggregate crushed to be continuously and evenly rolled small and large mixers of the rotary form continuously to be dried.

또한, 컨베이어 벨트 상에는 온도 센서가 구비되어 있어, 파쇄물의 건조 온도를 원하는 온도로 조절할 수 있고, 나아가 파쇄물 내의 잔존 수분의 양을 조절할 수 있다.In addition, a temperature sensor is provided on the conveyor belt, so that the drying temperature of the crushed material can be adjusted to a desired temperature, and further, the amount of moisture remaining in the crushed material can be adjusted.

본 발명의 아스콘은 상온 아스콘으로써, 전술한 재생골재를 사용하고 상기 재생골재는 수분이 잔존하기 때문에, 재생골재의 주성분인 콘크리트의 성분이 수분에 반응하여 다짐시 더욱 집결됨으로써 우수한 강도를 갖는다. 또한, 상기 아스콘의 혼합시 별도의 채움재를 사용하지 않고, 비가열 아스팔트와 다이머산만을 재생골재 및 기타 신규 골재와 혼합함으로써 아스콘 혼합 과정이 단순하며 경제적인 측면에서 매우 효율적이다.Ascon of the present invention is a room temperature ascone, because the above-mentioned recycled aggregate is used, and the recycled aggregate retains moisture, and thus has excellent strength as the components of concrete, which are the main components of the recycled aggregate, are further collected when compacted in response to moisture. In addition, the ascon mixing process is simple and economically effective by mixing only non-heated asphalt and dimer acid with recycled aggregates and other new aggregates without using a separate filler when mixing the ascon.

한편, 상기 재생골재를 이루는 콘크리트 파쇄물 내에 적정량의 수분이 포함될 경우, 상온 아스콘을 시공하기 전 보관 시 아스콘 혼합물 내의 용재가 침투하는 것을 방지함으로써, 골재가 굳어지지 않게 한다. 즉, 재생골재 내의 수분이 용제의 침투를 막는 보호수단으로 기능하며, 이를 통하여 아스콘의 보관성 및 작업 안정성을 현저히 증가시킬 수 있다.On the other hand, when the appropriate amount of water is included in the concrete crushing to form the recycled aggregate, by preventing the penetration of the material in the ascon mixture during storage before the construction of room temperature ascon, the aggregate is not hardened. In other words, the moisture in the recycled aggregate serves as a protective means to prevent the penetration of the solvent, through which can significantly increase the storage and work stability of ascon.

본 발명의 상온 아스콘은 안정도, 흐름값, 수침잔류안정도 등의 물성 면에서 신규골재를 이용한 기존 제품 대비 우수한 물성을 나타낼 수 있다. 결국, 본 발명에 따르면 상온 아스콘의 단가는 낮추고 물성은 극대화할 수 있어 향후 아스콘 분야의 경제성을 획기적으로 개선할 수 있을 것으로 기대하고 있다. Room temperature ascon of the present invention may exhibit superior physical properties compared to existing products using new aggregates in terms of physical properties such as stability, flow value, immersion residue stability. As a result, according to the present invention, it is expected that the unit cost of the room temperature ascon can be lowered and the physical properties can be maximized, thereby significantly improving the economics of the ascon field in the future.

도 1은 본 발명의 일 실시예에 따른 폐콘크리트 파쇄물의 건조 단계에서 사용되는 재생골재 건조장치를 개념적으로 도시한 개념도이다. 1 is a conceptual diagram conceptually showing a recycled aggregate drying apparatus used in the drying step of the waste concrete crushed material according to an embodiment of the present invention.

이하 첨부된 도면을 참조하여, 본 발명의 일 실시예에 재생골재의 제조방법을 자세하게 설명하도록 한다. 그러나 하기 설명은 본 발명을 개념적으로 이해하기 위한 설명들일뿐 아래 설명들에 의하여 본 발명의 기술사상이 제한되지 않는다. 본 발명의 기술사상은 오직 후술하는 청구범위에 의하여 해석되거나 제한될 수 있다. Hereinafter, with reference to the accompanying drawings, it will be described in detail a method for producing a recycled aggregate in one embodiment of the present invention. However, the following description is only for the conceptual understanding of the present invention is not limited by the following description. The spirit of the present invention may be interpreted or limited only by the following claims.

본 발명의 일 실시예에 따른 재생골재의 제조방법은 재생골재로서, 폐콘크리트를 사용한다. 폐콘크리트는 골재성분 뿐만 아니라 콘크리트에 포함된 각종 채움재 및 콘크리트 혼합물에 포함된 결합재 등의 유용성분을 포함하기 때문에, 폐콘크리트를 골재로 사용할 경우, 기능성 성분까지 아스콘 혼합시 활용될 수 있는 장점이 있다. The method for producing recycled aggregates according to an embodiment of the present invention uses waste concrete as recycled aggregates. Since waste concrete contains useful components such as various fillers included in concrete and binders included in concrete mixtures as well as aggregate components, when waste concrete is used as aggregate, there is an advantage that it can be utilized when mixing ascon to functional components. .

재생골재를 제조하기 위해서는, 우선 폐콘크리트를 파쇄하는 단계를 거친다. 파쇄된 폐콘크리트 파쇄물은 1차적으로 공지된 다양한 선별 방법에 의하여 입자 선별됨으로써, 8mm이하의 크기를 갖도록 선별되는 과정을 거친다. 이어서, 선별된 파쇄물은 이물질 제거를 위하여 세척 과정을 거친다. 따라서 위 과정을 거친 파쇄물은 젖은 생태를 유지한다. 이후, 젖은 상태의 파쇄물은 건조 단계를 거치게 된다. In order to produce recycled aggregate, first, the waste concrete is crushed. The crushed waste concrete crushed is screened to have a size of 8 mm or less by screening the particles by various sorting methods known first. The screened debris is then washed to remove debris. Thus, the crushed waste product maintains the wet ecology. Thereafter, the wet debris is subjected to a drying step.

도 1은 본 발명의 일 실시예에 따른 폐콘크리트 파쇄물의 건조 단계에서 사용되는 재생골재 건조장치를 개념적으로 도시한 개념도이다. 도 1을 참조하여, 본 발명의 주요 공정인 건조 단계를 자세하게 설명하도록 한다. 1 is a conceptual diagram conceptually showing a recycled aggregate drying apparatus used in the drying step of the waste concrete crushed material according to an embodiment of the present invention. Referring to Figure 1, it will be described in detail the drying step of the main process of the present invention.

도 1을 참조하면, 세척된 폐콘크리트 파쇄물(5)은 소형 호퍼(미도시)에 담아 재료분리를 최소화 한 후, 재생골재 건조장치(1000)로 공급됨으로써 이송과 동시에 건조 과정을 시작한다. 파쇄물(5)은 컨베이어벨트(50)를 따라 이송되며 건조된다. Referring to FIG. 1, the washed waste concrete crushed material 5 is placed in a small hopper (not shown) to minimize material separation, and is then supplied to the recycled aggregate drying apparatus 1000 to start the drying process simultaneously with the transfer. The crushed material 5 is transported along the conveyor belt 50 and dried.

상기 재생골재 건조장치(1000)는 복수의 원적외선히터(400)를 포함한다. 상기 원적외선히터(400)는 컨베이어벨트(50) 상에 순차적으로 배치된다. 상기 원적외선히터(400)는 파쇄물(5)을 약 150℃ 이상까지 가열할 수 있다. 본 실시예에서, 원적외선히터(400)는 LPG 가스를 연료로하여 구동되며, 이를 위하여 상기 재생골재 건조장치(1000)는 LPG 탱크(110)를 포함한다. LPG 탱크(110)는 송풍기(120)와 연동되어 있고, 상기 LPG 가스는 관로(300)를 통하여 원적외선히터(400)에 공급된다. 원적외선히터(400)는 바람을 일으키지 않고 파쇄물(5)에 복사열을 가함으로써 건조 과정에서 분진 등이 날릴 염려가 없다. 원적외선히터(400)는 컨베이어벨트(50)의 이동 구간에 소정 간격 이격되어 주기적으로 배치될 수 있다. 한편, 상기 원적외선히터(400)는 가스의 공급량을 조절하여 가열량이 조절될 수 있고, 이를 통하여 파쇄물(5)의 건조 수준을 조절할 수 있다.The recycled aggregate drying apparatus 1000 includes a plurality of far infrared heaters 400. The far infrared heater 400 is sequentially disposed on the conveyor belt 50. The far infrared heater 400 may heat the crushed material 5 to about 150 ℃ or more. In this embodiment, the far-infrared heater 400 is driven by LPG gas as fuel, the recycle aggregate drying apparatus 1000 includes an LPG tank 110 for this purpose. LPG tank 110 is interlocked with the blower 120, the LPG gas is supplied to the far infrared heater 400 through the conduit (300). The far-infrared heater 400 does not cause wind and does not cause dust or the like in the drying process by applying radiant heat to the crushed material 5. The far infrared heater 400 may be periodically spaced apart from the predetermined interval in the moving section of the conveyor belt (50). On the other hand, the far-infrared heater 400 may be controlled by adjusting the amount of supply of gas, thereby adjusting the drying level of the crushed material (5).

송풍기(120)는 LPG 가스의 유량 및 속도 등을 제어할 수 있는 콘트롤 박스(220)에 연결되어 있으며, 상기 콘트롤 박스(220)는 도 1에 도시된 온도센서(700)로부터 측정되는 파쇄물(5)의 온도 등을 입력받아 LPG 가스의 유량 및 속도를 조절하고 궁극적으로 파쇄물(5) 자체의 온도를 작업자의 의도대로 조절할 수 있도록 한다. 상기 콘트롤 박스(220)는 전력소스(210)로부터 전력을 공급받아 구동한다.Blower 120 is connected to a control box 220 that can control the flow rate and speed of the LPG gas, the control box 220 is a shredded material (5) measured from the temperature sensor 700 shown in FIG. In order to control the flow rate and speed of the LPG gas by inputting the temperature of) and ultimately, the temperature of the crushed material 5 itself can be adjusted according to the intention of the operator. The control box 220 is driven by receiving power from the power source 210.

컨베이어벨트(50)로 이송된 파쇄물(5)은 최초 젖은 상태로 이동하면서 원적외선히터(400)에 의하여 지속적으로 열을 공급받아 파쇄물(5) 입자 내부까지 건조시킨다. 또한, 컨베이어벨트(50) 상에서 이송되는 과정에서 혼합기(510, 520)에 의하여 고르게 펴지거나 굴려짐으로써 파쇄물(5)은 전체적으로 균일하게 건조될 수 있다. 즉, 불규칙한 건조에 의하여 파쇄물(5) 부위별로 수분함량이 현저히 차이가 나지 않도록 관리될 필요가 있는 것이다. 상기 혼합기(510, 520)는 대형 혼합기(510) 및 소형 혼합기(520)를 포함한다. 따라서 미분 ~ 8mm 이하의 분포를 갖는 파쇄물(5) 입자들을 고르게 혼합시킬 수 있다. 상기 혼합기(510, 520)는 로터리 형태의 혼합기로서, 톱니바퀴 형태나 볼트 형태를 가질 수 있다.The crushed material 5 transferred to the conveyor belt 50 is continuously supplied to the wetted state by the far-infrared heater 400 while moving to the wet state and dried to the inside of the crushed material 5 particles. In addition, the crushed material 5 may be uniformly dried as a whole by being evenly spread or rolled by the mixers 510 and 520 in the process of being transported on the conveyor belt 50. That is, it is necessary to be managed so that the moisture content of each of the shreds 5 is not significantly different due to irregular drying. The mixers 510, 520 include a large mixer 510 and a small mixer 520. Therefore, it is possible to evenly mix the particles of the crushed material 5 having a distribution of fine powder ~ 8 mm or less. The mixers 510 and 520 are rotary type mixers and may have a gear shape or a bolt shape.

컨베이어벨트(50)를 이동하면서 원적외선히터(400)를 경유한 후 온도센서(700)에 의하여 온도를 측정할 경우 복사열에 의하여 가열된 고온의 공기에 의하여 파쇄물(5) 자체의 온도가 정확하게 측정되기 어려운 면이 있다. 따라서 상기 재생골재 건조장치는 온도센서(700)에 파쇄물(5)이 도달하기 전에 열반사기(600)를 경유하도록 열반사기(600)를 포함한다. 상기 열반사기(600)는 파쇄물(5)이 열반사기(600)를 경유하면서 파쇄물(5) 자체의 열이 지속적으로 반사될 수 있도록 하는 역할을 한다. 따라서 이후 온도센서(700)는 파쇄물(5) 자체의 열과 평형인 공기의 온도를 측정함으로써 실질적으로 파쇄물(5) 자체의 건조 온도를 측정할 수 있다.When measuring the temperature by the temperature sensor 700 after passing through the far infrared heater 400 while moving the conveyor belt 50, the temperature of the crushed material 5 itself is accurately measured by the hot air heated by radiant heat. There is a difficult side. Therefore, the recycled aggregate drying apparatus includes a heat reflector 600 to pass through the heat reflector 600 before the crushed material 5 reaches the temperature sensor 700. The heat reflector 600 serves to allow the shredder 5 to continuously reflect the heat of the shredder 5 itself while passing through the heat reflector 600. Therefore, the temperature sensor 700 can then substantially measure the drying temperature of the shreds 5 itself by measuring the temperature of the air in equilibrium with the heat of the shreds 5 itself.

건조 파쇄물(5)의 온도는 40 내지 50℃로 유지되는 것이 바람직하다. 이러한 온도 조건으로 건조된 건조 파쇄물(5)의 잔존 수분의 함량은 후속 아스콘 혼합 과정의 작업성 및 아스콘의 물성을 극대화 할 수 있는 핵심요소로 작용할 수 있다. It is preferable that the temperature of the dry crushed material 5 is maintained at 40-50 degreeC. The residual moisture content of the dried crushed material 5 dried at such a temperature condition may act as a key factor in maximizing the workability and the properties of ascone in the subsequent ascon mixing process.

즉, 상기 재생골재 건조장치(1000)는 효과적으로 파쇄물(5)을 건조시킬 뿐만 아니라 궁극적으로 파쇄물(5) 내의 수분함량을 조절하는 장치로서 이후 아스콘 제조과정 및 제조되는 아스콘의 물성에 중요한 영향을 미치게 된다. That is, the recycled aggregate drying apparatus 1000 is an apparatus that not only dries the crushed material 5 effectively but also ultimately controls the water content in the crushed material 5 to thereby have an important influence on the production process of ascon and the physical properties of the produced ascon. do.

이렇게 준비된 재생골재는 아스콘 혼합에 사용된다. 본 발명에 따른 아스콘은 상온 아스콘이며, 통상 상온 아스콘은 골재, 채움재, 결합재 및 박리방지제를 포함하는 조성물이다. The recycled aggregate thus prepared is used for ascon mixing. Ascon according to the present invention is a room temperature ascon, usually a room temperature ascon is a composition comprising an aggregate, a filler, a binder and a peeling inhibitor.

그러나 본 발명에 따른 상온 아스콘은 혼합 과정에서 채움재 등이 배제될 수 있다. 이는 재생골재를 이루는 폐 콘크리트 자체에 이미 채움재 등의 성분이 포함되어 있기 때문이다. 또한, 콘크리트 혼합과정에서 배합된 다양한 결합재 등의 성분이 재생골재에 잔존하고 있기 때문에 아스콘 혼합 과정의 첨가물을 최소화할 수 있다. However, the room temperature ascon according to the present invention may be excluded from the filling material in the mixing process. This is because waste concrete itself, which forms the recycled aggregate, already contains components such as filler. In addition, since components such as various binders blended in the concrete mixing process remain in the recycled aggregate, additives in the ascon mixing process can be minimized.

본 발명의 일 실시예에 따른 상온 아스콘은, 재생골재, 신골재, 결합재로서 비가열 아스팔트 및 박리 방지제로서 다이머산만을 포함하며 별도의 첨가제 또는 기능제를 포함하지 않는다. 구체적으로 상기 상온 아스콘은 전술한 바에 의하여 제조된 8mm 이하의 크기를 갖는 재생골재 50 내지 90 중량%; 4 내지 8mm의 크기를 갖는 신골재 10 내지 50 중량%; 비가열 아스팔트 4 내지 10 중량%; 및 다이머산 0.04 내지 1.5 중량%를 포함한다. Room temperature ascone according to an embodiment of the present invention, recycled aggregate, new aggregate, non-heated asphalt as a binder and only dimer acid as a peeling preventive agent and does not include a separate additive or functional agent. Specifically, the room temperature ascon is 50 to 90% by weight of the recycled aggregate having a size of 8 mm or less prepared as described above; 10 to 50% by weight of new aggregate having a size of 4 to 8mm; 4-10% by weight of unheated asphalt; And 0.04 to 1.5% by weight of dimer acid.

상기 아스팔트는 비가열 아스팔트라면 그 종류와 형태가 크게 제한되지 않으며, 예를 들어 스트레이트 아스팔트, 컷백 아스팔트, 유화 아스팔트, 개질 아스팔트 등이 있다. 개질 아스팔트는 아스팔트 포장의 내구성, 내유동성, 내마모성, 미끄럼저항성 등을 향상시킬 목적으로 아스팔트 물성을 개선시킨 것으로서, 통상적으로 SBS, SBR과 같은 고무 또는 폴리에틸렌, 폴리프로필렌과 같은 플라스틱이 첨가된다. 본 발명에 따른 상온 아스콘의 일 성분인 결합재로는 컷백 아스팔트인 것이 바람직하다. 도로포장에 사용되는 아스팔트 시멘트는 상온에서 반고체 상태를 띠므로 다른 골재(骨材)와 혼합하거나 노면에 뿌릴 때면 반드시 가열하여 녹여서 사용해야만 했다. 이런 불편함을 줄이기 위해 아스팔트 시멘트를 휘발성의 석유 용제와 섞어서 액체 상태로 만든 것이 컷백 아스팔트이다. 컷백 아스팔트는 어떤 용제를 혼합하는가에 따라 증발하여 건조, 경화되는 속도가 달라지는데 급속경화형(rapid curing:RC), 중속경화형(medium curing:MC), 완속경화형(slow curing:SC)으로 구분된다. 급속경화형은 가솔린을 사용한 것으로 점도를 떨어뜨리고 유동성을 좋게 하며, 중속경화형은 등유를 사용하여 증발 속도를 적당히 늦추어 제조한 것이고, 완속경화형은 경유 등 중질유를 사용한 것을 말한다.If the asphalt is a non-heated asphalt, the type and shape thereof are not particularly limited, and examples thereof include straight asphalt, cutback asphalt, emulsified asphalt, and modified asphalt. Modified asphalt is to improve the asphalt physical properties for the purpose of improving the durability, flow resistance, wear resistance, slip resistance, etc. of the asphalt pavement, rubber, such as SBS, SBR or plastics such as polyethylene, polypropylene is usually added. As a binder of one component of room temperature ascon according to the present invention, it is preferable that the cutback asphalt. Asphalt cement used for road paving is semisolid at room temperature, so it must be heated and melted when mixed with other aggregates or sprayed on road surfaces. To reduce this inconvenience, cutback asphalt is made by mixing asphalt cement with a volatile petroleum solvent in a liquid state. Cutback asphalt is evaporated, dried, and cured at different speeds depending on which solvent is mixed. Rapid cut asphalt is classified into rapid curing (RC), medium curing (MC), and slow curing (SC). Rapid curing type uses gasoline to reduce viscosity and improve fluidity. Medium-speed curing type is produced by using kerosene to slow the evaporation rate, and slow curing type refers to using heavy oil such as diesel.

상온 아스콘에서 결합재로 사용되는 컷백 아스팔트는 통상적으로 침입도가 60~150인 스트레이트 아스팔트에 적당한 휘발성 용제, 즉 희석유를 가하여 점도를 저하시켜 유동성을 좋게 한 것으로서, 이때 희석유의 함량은 약 10~45 중량%이다. 컷백 아스팔트의 규격인 KSM2202에는 급속경화형 컷백 아스팔트를 점도의 정도에 따라 6등급(RC-0 부터 RC-5까지)으로 세분화하여 제품을 분류하고 있고, 주요 용도로 표면처리용 결합재, 개립도 골재로서 노상혼합공사용 결합재, 개립도 골재로서 상온보수공사 혼합물용 결합재, 개립도 골재로서 상온포설공사 기계혼합용 결합재, 찬 기후 조건하에서 상온포설공사 기계혼합용 결합재를 예시하고 있다. 또한, 컷백 아스팔트의 규격인 KSM2202에는 중속경화형 컷백 아스팔트를 점도의 정도에 따라 6등급(MC-0 부터 MC-5까지)으로 세분화하여 제품을 분류하고 있고, 주요 용도로 표면처리용 결합재, 개립도 골재로서 노상혼합공사용 결합재, 개립도 골재로서 상온보수공사 혼합물용 결합재, 프라임용 (Priming), 밀입도 골재로서 노상혼합공사용 결합재, 밀입도 골재로서 상온보수공사 혼합물용 결합재, 밀입도 골재로서 상온포설공사 기계혼합용 결합재를 예시하고 있다. 본 발명에 따른 상온 아스콘의 일 성분인 결합재로 사용되는 컷백 아스팔트는 아스콘이 사용되는 용도(차도 포장 또는 포수, 보도 포장 또는 보수, 터널 포장 또는 보수, 표층용, 중간층용, 기층용 등)에 따라 자유롭게 선택되어 사용될 수 있다.Cutback asphalt used as a binder in room temperature asphalt concrete is a good viscosity to improve the fluidity by adding a suitable volatile solvent, that is, diluent oil, to straight asphalt having a penetration of 60 to 150, and the dilution oil content is about 10 to 45 Weight percent. KSM2202, the standard for cutback asphalt, classifies products by classifying rapid curing cutback asphalt into 6 grades (RC-0 to RC-5) according to the degree of viscosity. Examples of binders for road-flood mixing, binders for room-temperature repair construction as open-end aggregates, binders for room-temperature laying construction as open-end aggregates, and binders for room-mix laying under cold climatic conditions. In addition, KSM2202, a cutback asphalt standard, classifies products by classifying medium-speed hardened cutback asphalt into six grades (MC-0 to MC-5) according to the degree of viscosity. Binders for road-mixing works as aggregates, Binders for room-temperature repair works as pavement aggregates, Primings, Binders for road-mixing works as aggregates, Binders for room-temperature repair work mixtures as aggregates, and at room temperature Illustrates binders for construction machinery mixing. Cutback asphalt used as a binder as a component of room temperature ascon according to the present invention, depending on the application (as well as road pavement or catcher, sidewalk pavement or repair, tunnel pavement or repair, surface layer, intermediate layer, base layer, etc.) It can be freely selected and used.

상기 박리방지제로서는 본 발명의 경우, 다이머산 단독으로 사용해도 전혀 물성 저하가 없다. 상기 다이머산은 아스팔트의 골재 면이 젖어 있을 때 부착을 좋게 함과 동시에 한번 부착한 아스팔트가 외력이나 비 등의 작용에 의해 벗겨지는 것을 방지하는 성분으로서 아스콘의 저항력을 증대시키는 역할을 한다. As said peeling inhibitor, even in the case of this invention, even if it uses dimer acid alone, there is no physical property fall at all. The dimer acid improves the adhesion of asphalt when the aggregate surface of the asphalt is wet and at the same time prevents the asphalt from being peeled off by the action of external force or rain as a component to increase the resistance of ascon.

하기 표 1은 본 발명의 일 실시예에 따른 상온 아스콘의 조성을 나타낸 것이다. 상기 아스콘에 사용된 골재는 4 내지 8mm의 입자분포를 갖는 신규 골재와 8mm 이하의 입도분포를 갖는 재생골재(KSF2357 잔골재입도 만족)가 4:6의 중량비로 혼합된 혼합 골재이다. 또한, 사용된 골재는 입자 분포에 따라 함량비를 기재하였다. Table 1 shows the composition of room temperature ascone according to an embodiment of the present invention. The aggregate used in the asphalt concrete is a mixed aggregate having a new aggregate having a particle distribution of 4 to 8 mm and a recycled aggregate having a particle size distribution of 8 mm or less (satisfactory KSF2357 fine aggregate particle size) in a weight ratio of 4: 6. In addition, the aggregate used described the content ratio according to the particle distribution.

8~5mm8-5mm 5~2.5mm5 ~ 2.5mm 2.5~
1.2mm
2.5 ~
1.2 mm
1.2~
0.6mm
1.2 ~
0.6mm
0.6~
0.3mm
0.6 ~
0.3mm
0.3~
0.15mm
0.3 ~
0.15mm
0.15~
0.08mm
0.15 ~
0.08mm
0.08mm
이하
0.08mm
Below
컷백
아스팔트
cutback
asphalt
다이머산Dimer Mountain
5~20%5-20% 40~70%40-70% 5~20%5-20% 3~10%3 ~ 10% 1~5%1-5% 1~5%1-5% 1~5%1-5% 1~5%1-5% 4~10%4-10% 0.04~
1.5%
0.04-
1.5%

물성평가Property evaluation

하기 표 2는 종래 신규 골재를 사용한 출원인 기존제품(다현산업)과 상기 표 1의 조성으로 제조된 아스콘 제품에 대하여 물성 시험(KSF2369 기준)한 결과를 기재한 표이다. Table 2 is a table showing the results of the physical property test (based on KSF2369) for the conventional products (Dahyun Industry) and the Ascon products manufactured with the composition of Table 1 using the new novel aggregate.

구분division 출원인 기존제품Applicant Existing Product 재생골재 사용 제품Recycled Aggregate Used Products 안정도(N)Stability (N) 3,0003,000 5,5005,500 흐름값(1/10mm)Flow value (1 / 10mm) 2727 3030 수침잔류안정도(%)Immersion Residual Stability (%) 80%80% 98%98%

표 2를 참조하면, 재생골재의 주성분인 콘크리트의 성분이 수분에 반응하고 다짐 시 더욱 집결되어 우수한 강도가 측정된다. 기존제품대비 안정도가 70%이상 상승하였으며 수침잔류안정도 또한 95%이상 만족하는 결과를 얻을 수 있었다.Referring to Table 2, the components of the concrete, the main component of the recycled aggregates reacts to moisture and is further collected when compacted to measure excellent strength. The stability was more than 70% compared to the existing product, and the stability of immersion residue was also more than 95%.

Claims (5)

콘크리트 폐기물을 파쇄하고 크기를 선별하여 재생골재용 파쇄물을 준비하는 단계;
상기 파쇄물을 세척하는 단계; 및
콘크리트의 다짐시 집결성을 증가시키고, 상온 아스콘을 보관시 아스콘 혼합물 내의 용제가 침투하는 것을 방지하기 위한 보호수단을 형성하기 위하여, 세척된 젖은 상태의 파쇄물을 복수의 원적외선 히터가 구비된 컨베이어 벨트에 순차적으로 적재하여 이송하면서 수분을 조절하는 단계; 를 포함하는,
상온 아스콘용 재생골재의 제조방법.
Crushing concrete waste and screening the size to prepare shredded material for recycled aggregate;
Washing the debris; And
In order to increase the cohesiveness when compacting concrete and to form a protective means for preventing the penetration of the solvent in the ascon mixture when storing the room temperature ascon, the washed wet crushed matter is placed on a conveyor belt equipped with a plurality of far infrared heaters. Controlling moisture while loading and transporting sequentially; Including,
Method for producing recycled aggregate for room temperature ascon.
제1항에 있어서,
상기 파쇄물은 8mm 이하의 크기로 선별되는 것을 특징으로 하는 상온 아스콘용 재생골재의 제조방법.
The method of claim 1,
The crushed product is a method for producing a recycled aggregate for room temperature ascon characterized in that the screening is selected in size less than 8mm.
제1항에 있어서,
상기 건조된 재생골재의 온도가 40 내지 50℃의 온도가 되도록 원적외선 히터의 발열량을 조절하는 것을 특징으로 하는 상온 아스콘용 재생골재의 제조방법.
The method of claim 1,
Method for producing a recycled aggregate for room temperature ascone, characterized in that for controlling the calorific value of the far-infrared heater so that the temperature of the dried recycled aggregate is 40 to 50 ℃.
i) 콘크리트 폐기물을 파쇄하고 크기를 선별하여 재생골재용 파쇄물을 준비하는 단계; 상기 파쇄물을 세척하는 단계; ii) 콘크리트의 다짐시 집결성을 증가시키고, 상온 아스콘을 보관시 아스콘 혼합물 내의 용제가 침투하는 것을 방지하기 위한 보호수단을 형성하기 위하여, 세척된 젖은 상태의 파쇄물을 40 내지 50℃의 온도로 유지하도록 복수의 원적외선 히터가 구비된 컨베이어 벨트에 순차적으로 적재하여 이송하면서 파쇄물의 수분을 조절하는 단계; 및 iii) 파쇄물의 입도가 8mm 이하가 되도록 선별하는 단계를 포함하는 상온 아스콘용 재생골재의 제조단계; 및
상기 재생골재와 4 내지 8mm의 입도분포를 갖는 신규골재를 혼합하는 단계를 포함하는 것을 특징으로 하는 상온 아스콘의 제조방법.
i) crushing the concrete waste and screening the size to prepare shreds for recycled aggregate; Washing the debris; ii) to maintain the wet wet shreds at a temperature of 40-50 ° C. in order to increase the cohesiveness when compacting concrete and to form a protective means for preventing the penetration of solvent in the ascon mixture when storing the room temperature ascon Controlling moisture of the crushed product while sequentially loading and transporting the conveyor belt equipped with a plurality of far infrared heaters so as to transfer the same; And iii) the step of producing a recycled aggregate for room temperature ascon including the step of selecting the particle size of the crushed to 8mm or less; And
Method for producing a room temperature ascon characterized in that it comprises the step of mixing the aggregate and the new aggregate having a particle size distribution of 4 to 8mm.
제4항의 방법으로 제조되고,
5,500의 안정도(N), 30의 흐름값(1/10mm) 및 98%의 수침잔류안정도를 갖는 것을 특징으로 하는 상온 아스콘.
Prepared by the method of claim 4,
Room temperature ascon characterized in that it has a stability (N) of 5,500, a flow value of 30 (1 / 10mm) and a immersion residual stability of 98%.
KR1020190074044A 2019-06-21 2019-06-21 Method of manufacturing recycled aggregate and normal temperature ascon manufactured by using the same KR102213683B1 (en)