KR20060074068A - Pre coated metal coating polyester resin and method of preparing the same - Google Patents

Pre coated metal coating polyester resin and method of preparing the same Download PDF

Info

Publication number
KR20060074068A
KR20060074068A KR1020040112688A KR20040112688A KR20060074068A KR 20060074068 A KR20060074068 A KR 20060074068A KR 1020040112688 A KR1020040112688 A KR 1020040112688A KR 20040112688 A KR20040112688 A KR 20040112688A KR 20060074068 A KR20060074068 A KR 20060074068A
Authority
KR
South Korea
Prior art keywords
glycol
polyester resin
acid
mixture
pcm
Prior art date
Application number
KR1020040112688A
Other languages
Korean (ko)
Other versions
KR100644766B1 (en
Inventor
김상곤
정태섭
Original Assignee
(주)디피아이 홀딩스
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by (주)디피아이 홀딩스 filed Critical (주)디피아이 홀딩스
Priority to KR1020040112688A priority Critical patent/KR100644766B1/en
Publication of KR20060074068A publication Critical patent/KR20060074068A/en
Application granted granted Critical
Publication of KR100644766B1 publication Critical patent/KR100644766B1/en

Abstract

도장후 내약품성, 내습성이 우수하며, 특히 가공성이 우수한 PCM 도료용 폴리에스테르 수지 조성물이 개시되어 있다. PCM 도료용 폴리에스테르 수지는 글리콜 총 당량에 대하여 1,3-사이클로헥산디메탄올과 1,4-사이클로헥산디메탄올 혼합된 제1 글리콜 5 내지 40%와 제2 글리콜 60 내지 95%를 포함하는 글리콜 혼합물과 아로마틱산, 알리파틱산 또는 이들의 혼합물을 포함하는 2가산 혼합물이 1.0: 1.0 내지 1.1 당량비로 축합되어 형성된다. 상기 열경화성 PCM 도료용 폴리에스테르 수지 조성물은 상도 및 소지에 대한 밀착성이 우수하고, 특히 가공성이 우수하다.Disclosed is a polyester resin composition for PCM coatings having excellent chemical resistance and moisture resistance after coating, and particularly excellent workability. The polyester resin for PCM coating is a glycol comprising 5 to 40% of the first glycol and 60 to 95% of the second glycol mixed with 1,3-cyclohexanedimethanol and 1,4-cyclohexanedimethanol based on the total equivalent weight of glycol. A diacid mixture comprising a mixture and an aromatic acid, aliphatic acid or a mixture thereof is formed by condensation in a ratio of 1.0: 1.0 to 1.1 equivalents. The polyester resin composition for thermosetting PCM paint is excellent in adhesion to the top coat and the base, and particularly excellent in workability.

Description

피씨엠 도료용 폴리에스테르 수지 및 그 제조 방법{PRE COATED METAL COATING POLYESTER RESIN AND METHOD OF PREPARING THE SAME}Polyester resin for PCM paint and its manufacturing method {PRE COATED METAL COATING POLYESTER RESIN AND METHOD OF PREPARING THE SAME}

본 발명은 폴리에스테르 수지 및 그 제조방법에 관한 것으로, 보다 상세하게는 가전용 PCM(Pre Coated Metal) 강판의 하도용 도료 조성물로 사용되는 PCM 도료용 폴리에스테르 수지 및 그 제조 방법에 관한 것이다.The present invention relates to a polyester resin and a method for manufacturing the same, and more particularly, to a polyester resin for PCM paint used as a coating composition for the coating of the PCM (Pre Coated Metal) steel sheet for home appliances, and a method for producing the same.

일반적으로 사용되는 PCM 강판 도장용 수지 조성물은 아크릴계, 우레탄계, 에폭시계, 폴리에스테르계, 실리콘계, 불소계, 폴리염화계 등으로 다양하다. 도료의 대부분은 열경화성이며, 특수한 도료의 물성을 요구하는 제품이외에는 폴리에스테르계와 에폭시계 수지 조성물이 많이 사용되며, 그 중에서도 특히 폴리에스테르 수지를 이용한 도료가 가장 많이 사용된다.Resin compositions for PCM steel sheet coating generally used are acrylic, urethane, epoxy, polyester, silicone, fluorine, polychlorinated and the like. Most of the paint is thermosetting, except for a product that requires the properties of special paints, polyester and epoxy resin compositions are used a lot, and in particular, paints using a polyester resin is most used.

PCM 강판의 하도에 도장하는 도료의 수지 조성물에는 다음과 같은 물성이 요구된다. 첫째, 도장후 소지 또는 상도와의 밀착성, 유연성 정도를 나타내는 가공성, 내마찰 MEK(methyl ethyl ketone)성 등과 같은 기계적 물성과 둘째, 내산성, 내알카리성, 내후성등의 화학적 물성 등이 그것이다. 이에 더하여, 생산성 및 코스트가 좌우되는 작업성 등도 우수해야 된다.The following physical properties are calculated | required by the resin composition of the coating material coat | covered by the undercoat of a PCM steel plate. First, mechanical properties such as adhesion to the base or top coat after coating, degree of flexibility, mechanical resistance such as friction MEK (methyl ethyl ketone), and second, chemical properties such as acid resistance, alkali resistance and weather resistance. In addition, productivity and cost dependability and workability should also be excellent.

지금까지 사용되고 있는 PCM 강판 하도 도장용 수지 조성물에는 폴리에스테르계와 에폭시계가 주종을 이루고 있다. PCM 강판 하도용 폴리에스테르 도료는 상도 도장 후 가공성이 우수하고 그 밖의 내약품성, 작업성 등은 우수하지만 상도 또는 소지와의 밀착성이 불량하여 스크레치성이 취약한 문제점이 있다. The resin composition for undercoat coating of PCM steel plate used so far is mainly a polyester type and an epoxy type. Polyester coating for PCM steel plate undercoat is excellent in workability after top coat and other chemical resistance, workability, etc., but poor scratchability due to poor adhesion to the top coat or the base.

또한 PCM 강판 하도용 에폭시도료는 상도 또는 소지와의 밀착성이 특히 우수하여 스크레치성은 우수하지만 가공성이 폴리에스테르계 도료보다 불량한 문제점이 있다. 따라서 그 동안은 위와 같은 폴리에스테르계 및 에폭시계 하도용 도료의 상반되는 물성 차이 때문에 PCM 강판 하도용 도료에는 사용되는 수지를 고려하여 사용해야 하는 어려움을 갖는다.In addition, the epoxy coating for PCM steel plate undercoat is particularly excellent in adhesion to the top coat or the base material has excellent scratch resistance but poor workability than polyester-based paint. Therefore, in the meantime, due to the difference in the physical properties of the polyester-based and epoxy-based paint for coating as described above, there is a difficulty that should be used in consideration of the resin used in the paint for PCM steel coating.

따라서, 상술한 문제점을 해결하기 위한 본 발명의 제1 목적은 소지 또는 상도와의 밀착성, 내습성등을 향상시키고, 에폭시계 수지 조성물의 문제점인 낮은 가공성을 향상시킬 수 있는 PCM 도료용 폴리에스테르 수지를 제공하는데 있다. Therefore, the first object of the present invention for solving the above problems is to improve the adhesion, moisture resistance and the like to the base or top, polyester resin for PCM coatings that can improve the low workability which is a problem of the epoxy resin composition To provide.

또한, 본 발명의 제 2목적은 상기한 물성을 갖는 PCM 도료용 폴리에스테르 수지의 제조 방법을 제공하는데 있다.In addition, a second object of the present invention is to provide a method for producing a polyester resin for PCM paint having the above-described physical properties.

상기 제1 목적을 달성하기 위한 본 발명의 일 실시예에 따른 PCM 도료용 폴리에스테르 수지는 글리콜 총 당량에 대하여 1,3-사이클로헥산디메탄올과 1,4-사이클로헥산디메탄올 혼합된 제1 글리콜 5 내지 40%와 제2 글리콜 60 내지 95%를 포함하는 글리콜 혼합물 및 아로마틱산, 알리파틱산 또는 이들의 혼합물을 포함하는 2 가산 혼합물이 1.0:1.0 내지 1.1 당량비로 축합되어 형성된다.PCM paint polyester resin according to an embodiment of the present invention for achieving the first object is a first glycol mixed with 1,3-cyclohexanedimethanol and 1,4-cyclohexanedimethanol based on the total glycol equivalent A glycol mixture comprising 5-40% and 60-95% of the second glycol and a diacid mixture comprising aromatic acids, aliphatic acids or mixtures thereof are formed condensed in a ratio of 1.0: 1.0 to 1.1 equivalents.

또한, 상기 제 2목적을 달성하기 위한 본 발명의 일 실시예에 따른 PCM 도료용 폴리에스테르 수지의 제조방법에 있어서, 글리콜 총 당량에 대하여 1,3-사이클로헥산디메탄올과 1,4-사이클로헥산디메탄올 혼합된 제1 글리콜 5 내지 40%와 제2 글리콜 60 내지 95%를 포함하는 글리콜 혼합물을 형성한다. 이어서, 아로마틱산, 알리파틱산 또는 이들의 혼합물을 포함하는 2가산 혼합물을 형성한다. 이어서, 상기 글리콜 혼합물과 상기 2가산 혼합물을 1.0: 1.0 내지 1.1 당량비로 축합 반응시킴으로서 열경화성 폴리에스테르 수지가 제조된다.In addition, in the method for producing a polyester resin for PCM paint according to an embodiment of the present invention for achieving the second object, 1,3-cyclohexanedimethanol and 1,4-cyclohexane relative to the total equivalent glycol A glycol mixture comprising 5-40% of the first glycol mixed with 60-95% of the second glycol is formed. Subsequently, a diacid mixture comprising an aromatic acid, aliphatic acid or a mixture thereof is formed. Subsequently, the thermosetting polyester resin is prepared by condensing the glycol mixture and the diacid mixture in a ratio of 1.0: 1.0 to 1.1 equivalents.

이에 따른 본 발명의 PCM 도료용 폴리에스테르 수지 및 그 제조 방법은 PCM 강판 하도용 도료로 사용되는 기존 폴리에스테르계 도료의 내습성 부족, 소지 및 상도와의 밀착성이 불량한 문제점과 에폭시계 도료의 가공성이 불량한 문제점을 해결할 수 있다. 즉, 도료의 가공성과 상도와의 밀착성, 내습성을 향상시킨 열 경화성의 PCM 도료용 폴리에스테르 수지 조성물을 제공할 수 있다.Accordingly, the polyester resin for PCM paint of the present invention and a method of manufacturing the same have problems of poor moisture resistance, poor adhesion to base material and top coat, and processability of epoxy-based paints of existing polyester paints used as PCM steel plate paints. Poor problem can be solved. That is, the polyester resin composition for thermosetting curable PCM coatings which improved the adhesiveness with the topability of a coating material, and moisture resistance can be provided.

이하, 본 발명을 더욱 상세히 설명하기로 한다.Hereinafter, the present invention will be described in more detail.

본 발명의 PCM 도료용 폴리에스테르 수지는 PCM 하도용 도료에 적용되는 열경화성 폴리에스테르 수지로서 1,3-사이클로헥산디메탄올과 1,4-사이클로헥산디메탄올 혼합된 제1 글리콜 5 내지 40%와 제2 글리콜 60 내지 95%를 포함하는 글리콜 혼합물과 아로마틱산, 알리파틱산 또는 이들의 혼합물을 포함하는 2가산 혼합물 축합반응하여 형성된다.The polyester resin for PCM paint of the present invention is a thermosetting polyester resin applied to PCM paint for coating, and 5 to 40% of first glycol mixed with 1,3-cyclohexanedimethanol and 1,4-cyclohexanedimethanol It is formed by the condensation reaction of a glycol mixture comprising 60 to 95% di glycol and a diacid mixture comprising aromatic acid, aliphatic acid or a mixture thereof.

먼저, 글리콜 화합물은 총 글리콜 당량에 대하여 제1 글리콜 5 내지 40%와 제2 글리콜 60 내지 95%가 혼합되어 있다. 상기 제1 글리콜은 하기와 같은 화학식 (1)으로 표기되는 1,3-사이클로헥산디메탄올(1,3-Cyclohexanedimethanol)과 하기 화학식 (2)으로 표기되는 1,4-사이클로헥산디메탄올(1,4-Cyclohexanedimethanol)이 1 : 1 (50%:50%)비율로 혼합된 구조를 갖는 글리콜 화합물이다. First, the glycol compound is a mixture of 5 to 40% of the first glycol and 60 to 95% of the second glycol relative to the total glycol equivalent. The first glycol is 1,3-cyclohexanedimethanol represented by the following formula (1) and 1,4-cyclohexanedimethanol represented by the following formula (2) (1, 4-Cyclohexanedimethanol) is a glycol compound having a structure in which the ratio is 1: 1 (50%: 50%).

Figure 112004061473368-PAT00001
------(1)
Figure 112004061473368-PAT00002
------(2)
Figure 112004061473368-PAT00001
------(One)
Figure 112004061473368-PAT00002
------(2)

상기 글리콜 화합물(혼합된(Mixed) 사이클로헥산디메탄올)은 수지합성시 용해도 및 반응성, 내약품성, 내습성등이 좋고, 네오펜틸 글리콜보다 고경도를 갖으며, 우수한 내산성, 향상된 내충격성, 유사한 유연성( Flexibility)을 갖는다. 또한 기존의 1,4-사이클로헥산디메탄올 보다 우수한 용해도, 저점도, 특히 유연성이 좋아 가공성 및 밀착성 증진에 도움이 되는 글리콜 화합물이다.The glycol compound (Mixed cyclohexane dimethanol) has good solubility and reactivity in the synthesis of resin, chemical resistance, moisture resistance, etc., has higher hardness than neopentyl glycol, excellent acid resistance, improved impact resistance, similar flexibility (Flexibility) In addition, it is a glycol compound that has good solubility, low viscosity, and particularly good flexibility than conventional 1,4-cyclohexanedimethanol, which helps to improve processability and adhesion.

상기 제 2 글리콜은 예컨대 사이클로헥산디메탄올, 에틸렌 글리콜, 프로필렌 글리콜, 메틸프로판디올, 네오펜틸 글리콜, 1,4-사이클로헥산디메틸올, 1,6-헥산디올, 에틸렌옥사이드가 부가된 비스페놀에이 등을 예로 들 수 있다. 이들은 단독 또는 혼합하여 사용할 수 있다.The second glycol is, for example, cyclohexanedimethanol, ethylene glycol, propylene glycol, methyl propanediol, neopentyl glycol, 1,4-cyclohexanedimethylol, 1,6-hexanediol, bisphenol A added with ethylene oxide, and the like. For example. These can be used individually or in mixture.

제1 글리콜 및 제2 글리콜을 포함하는 글리콜 혼합물은 총당량에서 제1 글리콜의 함량이 5% 미만이거나 제2 글리콜 함량이 95%를 초과할 경우 본 발명의 폴리 에스테르 수지를 포함하는 PCM 하도용 도료는 밀착성, 가공성, 내약품성, 내습성등이 떨어지는 문제점이 발생을 갖는다. 반면에 제1 글리콜의 함량이 40%를 초과하거나, 제2 글리콜의 함량이 60% 미만일 경우 PCM 하도용 도료 도막의 코인 스크레치성 및 MEK 러빙성등이 떨어지는 문제점이 발생한다.The glycol mixture comprising the first glycol and the second glycol is a PCM paint for coating comprising the polyester resin of the present invention when the total glycol content is less than 5% or the second glycol content is more than 95%. There is a problem that the adhesion, processability, chemical resistance, moisture resistance and the like is inferior. On the other hand, when the content of the first glycol is more than 40%, or the content of the second glycol is less than 60%, there is a problem that the coin scratchability and MEK rubbing property of the PCM coating material coating film falls.

따라서, 상기 글리콜 혼합물은 제1 글리콜을 5 내지 40%를 포함하고, 제2 글리콜을 60 내지 95%를 포함한다. 바람직하게는 상기 글리콜 혼합물은 제1 글리콜을 10 내지 35%를 포함하고, 제2 글리콜을 65 내지 90%를 포함한다.Thus, the glycol mixture comprises 5-40% of the first glycol and 60-95% of the second glycol. Preferably the glycol mixture comprises 10 to 35% of the first glycol and 65 to 90% of the second glycol.

또한, 본 발명의 PCM 도료용 폴리에스테르 수지를 제조하기 위해 적용되는 2가산 혼합물은 아로마틱산, 알리파틱산 또는 이들의 혼합물을 포함한다.In addition, the diacid mixture applied to prepare the polyester resin for PCM paint of the present invention includes an aromatic acid, aliphatic acid or a mixture thereof.

2가산 혼합물에 포함되는 아로마틱산은 예컨대 프탈릭 안하이드라이드, 테트라하이드로 프탈릭 안하이드라이드, 이소프탈릭산, 테레프탈릭산 등을 예를 들 수 있고, 이들은 단독 또는 혼합하여 사용한다. 상기 2가산에 포함되는 아리파틱산은 예컨대 세바식산, 아디픽산, 아젤릭산, 트리멜리틱 안하이드라이드 등을 예를 들 수 있고, 이들은 또는 혼합하여 사용한다.Examples of the aromatic acid contained in the diacid mixture include phthalic anhydride, tetrahydro phthalic anhydride, isophthalic acid, terephthalic acid, and the like, and these are used alone or in combination. The aliphatic acid contained in the diacid includes, for example, sebacic acid, adipic acid, azelic acid, trimellitic anhydride, and the like.

일반적으로, 상기 아로마틱산은 경도가 우수하나 유연성이 부족한 특성을 갖고, 상기 알리파틱산은 유연성은 우수하나 경도가 떨어지는 경향이 있다. 상기 도장용 조성물에서 목표하는 품질은 경도의 경우 연필경도가 F 이상인 것이 바람직하고 유연성, 즉 가공성의 경우 2T에 크랙이 발생하지 않는 정도인 것이 바람직한 것으로 보고 있다. In general, the aromatic acid has excellent hardness but lacks flexibility, and the aliphatic acid tends to have excellent flexibility but low hardness. The target quality in the coating composition is that it is preferable that the hardness of the pencil hardness F or more in the case of hardness, that is, the degree of cracking does not occur in 2T in the case of flexibility, namely workability.

따라서, 본 발명에서는 충분한 경도와 유연성을 발휘할 수 도로고 고경도의 아로마틱산과 유연성이 좋은 알리파틱 이가산을 적절히 조합된 2 가산 혼합물을 사용한다.Therefore, in the present invention, a biaddition mixture using an appropriate combination of high and high hardness aromatic acids and highly flexible aliphatic diacids can exhibit sufficient hardness and flexibility.

구체적으로는, 상기 2가산 혼합물은 프탈릭 안하이드라이드, 테트라하이드로 프탈릭 안하이드라이드, 이소프탈릭산, 테레프탈릭산로 이루어진 군에서 선택된 적어도 하나 아로마틱산이 2가산 총 당량의 50 내지 100%를 포함한다. 또한, 2가산 혼합물은 세바식산, 아디픽산, 아젤릭산로 이루어진 군에서 선택된 적어도 하나의 알리파틱산이 총 당량의 0 내지 50%를 포함한다.Specifically, the diacid mixture comprises 50 to 100% of the total equivalent of at least one aromatic acid selected from the group consisting of phthalic anhydride, tetrahydro phthalic anhydride, isophthalic acid and terephthalic acid. . In addition, the diacid mixture comprises 0-50% of the total equivalent of at least one aliphatic acid selected from the group consisting of sebacic acid, adipic acid, azelic acid.

따라서, 2가산 혼합물은 아로마틱산이 2가산 총 당량의 50 내지 100%를 포함하고, 알리파틱산이 2가산 총 당량의 0 내지 50%를 포함하는 것이 바람직하다. 아로마틱산 55 내지 95%를 포함하고, 알리파틱산이 2가산 혼합물 총 당량의 5 내지 45%를 포함하는 것이 보다 바람직하다.Thus, it is preferred that the diacid mixture comprises 50-100% of the total equivalent of diacid, and aliphatic acid comprises 0-50% of the total equivalent of diacid. It is more preferred that the aromatic acid comprises 55 to 95% and the aliphatic acid comprises 5 to 45% of the total equivalent of the diacid mixture.

본 발명의 글리콜 혼합물에 대하여 2가산 혼합물의 혼합 당량비가 1.0 : 1.0 미만일 경우 즉, 글리콜 혼합물의 함량이 2 가산 혼합물의 함량보다 많을 경우 상기 본말명의 폴리에스테르 수지를 포함하는 도료를 PCM 강판 하도에 도장시 소지 또는 상도와의 밀착성이 만족스럽지 못한 문제점을 갖게된다. 반면에 글리콜 혼합물에 대하여 2가산 혼합물의 혼합 당량비가 1.0 : 1.1을 초과 즉, 2가산 혼합물의 함량이 글리콜의 함량보다 10%를 초과할 경우 도장시 가공성과 내수성등의 내약품성이 불량하게 되는 문제점을 갖는다.When the mixing equivalent ratio of the diacid mixture is less than 1.0: 1.0 for the glycol mixture of the present invention, that is, when the content of the glycol mixture is more than the content of the diacid mixture, the paint containing the polyester resin of the above-mentioned real name is coated on the PCM steel plate under the coating. Adhesion with the substrate or the top coat is not satisfactory. On the other hand, when the mixing equivalence ratio of the diacid mixture is more than 1.0: 1.1 to the glycol mixture, that is, when the content of the diacid mixture is more than 10% of the glycol content, the chemical resistance such as processability and water resistance during coating becomes poor. Has

따라서, 상기 글리콜 혼합물과 2가산 혼합물은 혼합 당량비로 1.0 : 1.0 내지 1:1을 갖는 것이 바람직하고, 1.0: 1.0 내지 1.05의 혼합 당량비를 갖는 것이 보다 바람직하다.Accordingly, the glycol mixture and the diacid mixture preferably have a mixing equivalent ratio of 1.0: 1.0 to 1: 1, and more preferably a mixed equivalent ratio of 1.0: 1.0 to 1.05.

상기 본 발명의 PCM 도료용 폴리에스테르계 수지는 분자량은 PCM 도료용 폴리에스테르 수지는 하이드록시 값이 19 내지 21 이고, 산가가 5이하이고, 가드너 점도가 Z-Z3, 평균 분자량이 10,000 내지 35000을 갖는 것이 바람직하다. The polyester-based resin for PCM paint of the present invention has a molecular weight of the polyester resin for PCM paint has a hydroxy value of 19 to 21, an acid value of 5 or less, Gardner viscosity of Z-Z3, and an average molecular weight of 10,000 to 35000. It is desirable to have.

여기서, 상기 PCM 도료용 폴리에스테르계 수지 분자량이 10,000 미만일 경우에는 가공성 및 경도가 떨어지고, 분자량이 35,000을 초과할 경우에는 점성 및 작업성을 위해 적용되는 용제와의 상용성이 떨어져서 도료의 고체 함량이 낮아지고 이에 따라 PCM 라인의 고속 작업성이 떨어지기 문제점을 갖는다. 따라서, 상기 폴리에스테르계 수지의 분자량은 10,000 내지 35,000을 갖고 바람직하게는 분자량이 15000 내지 30,000을 갖는다.Here, when the molecular weight of the polyester-based resin for PCM paint is less than 10,000, workability and hardness are lowered, and when the molecular weight is more than 35,000, the solid content of the paint is lowered due to incompatibility with a solvent applied for viscosity and workability. There is a problem that the lower the high speed workability of the PCM line. Therefore, the molecular weight of the polyester resin has a 10,000 to 35,000 and preferably has a molecular weight of 15000 to 30,000.

PCM 도장용 폴리에스테르 수지 제조방법Manufacturing method of polyester resin for PCM coating

먼저, 글리콜 총 당량에 대하여 1,3-사이클로헥산디메탄올과 1,4-사이클로헥산디메탄올 혼합된 제1 글리콜 5 내지 40%와 제2 글리콜 60 내지 95%를 포함하는 글리콜 혼합물을 형성한다. 상기 제1 글리콜, 제2 글리콜 및 글리콜 혼합물에 대한 설명은 위에서 상세히 설명하였기 때문에 중복을 피하기 위해 생략한다.First, a glycol mixture comprising 5 to 40% of the first glycol and 60 to 95% of the second glycol mixed with 1,3-cyclohexanedimethanol and 1,4-cyclohexanedimethanol is formed based on the total equivalent glycol. Since the description of the first glycol, the second glycol and the glycol mixture has been described in detail above, it is omitted to avoid duplication.

이어서, 아로마틱산, 알리파틱산 또는 이들의 혼합물을 포함하는 2가산 혼합물을 형성한다. 상기 본 발명의 2 가산 혼합물은 형성되는 도료 도막의 충분한 경도와 유연성을 발휘할 수 있도록 고경도의 아로마틱산과 유연성이 우수한 알리파틱산을 적절히 조합하여 사용한다. 구체적으로는 2가산 혼합물은 아로마틱산이 2가산 총 당량의 50 내지 100%를 포함하고, 알리파틱산이 2가산 총 당량의 0 내지 50%를 포함하는 것이 바람직하다. 보다 바람직하게는 아로마틱산 55 내지 95%를 포함하고, 알리파틱산이 2가산 혼합물 총 당량의 5 내지 45%를 포함하는 것이 바람직하다.Subsequently, a diacid mixture comprising an aromatic acid, aliphatic acid or a mixture thereof is formed. The biadditive mixture of the present invention uses a combination of high hardness aromatic acid and aliphatic acid with excellent flexibility so as to exhibit sufficient hardness and flexibility of the coating film to be formed. Specifically, the diacid mixture preferably contains 50 to 100% of the total equivalent of diacid, and aliphatic acid comprises 0 to 50% of the total equivalent of diacid. More preferably, 55 to 95% of aromatic acids, and 5 to 45% of the total equivalent of the diacid mixture are preferred.

이어서, 상기 글리콜 혼합물과 상기 2가산 혼합물을 1.0: 1.0 내지 1.1당량비로 축합 반응시켜 열경화성 폴리에스테르 수지를 형성한다. 이와 같은 방법으로 형성된 PCM 도료에 적용되는 열결화성 폴리에스테르 수지는 하이드록시 값이 19 내지 21 이고, 산가가 5이하이고, 가드너 점도가 Z-Z3, 평균 분자량이 10,000 내지 35000인 것을 특성을 갖는다.Subsequently, the glycol mixture and the diacid mixture are condensed with each other in a ratio of 1.0: 1.0 to 1.1 equivalents to form a thermosetting polyester resin. The thermosetting polyester resin applied to the PCM paint formed by the above method has a hydroxy value of 19 to 21, an acid value of 5 or less, a Gardner viscosity of Z-Z3 and an average molecular weight of 10,000 to 35000.

이하, 본 발명의 구체적인 실시예 및 실험예를 통하여 본 발명을 상세히 설명하기로 한다. 그러나, 본 발명은 하기의 실시예 및 합성예로 한정되는 것이 아님은 물론이다.Hereinafter, the present invention will be described in detail through specific examples and experimental examples. However, the present invention is not limited to the following examples and synthesis examples, of course.

실시예 1Example 1

2ℓ4구 플라스크에 온도계, 응축기, 교반기 및 콘덴서를 설치하고 승온장치를 부착하였다. 여기에 네오펜틸글리콜 148g, 1,6-헥산디올 42g, 부틸렌 글리콜 129g, 사이클로헥산디메탄올 50g를 포함하는 글리콜 혼합물과 아디픽산 71g, 이소프탈릭산 486g를 포함하는 2 가산 혼합물을 투입한 후 서서히 교반하면서 240℃로 승온하였다. 이후, 약 7-8시간 동안 축합 반응을 수행하여 수산기값이 21, 산가가 5, 점도(가드너)가 Z-Z1인 열경화성 폴리에스테르 수지를 수득하였다.A 2-liter four-necked flask was equipped with a thermometer, condenser, stirrer and condenser and a temperature raising device was attached. To this was added a glycol mixture containing 148 g of neopentyl glycol, 42 g of 1,6-hexanediol, 129 g of butylene glycol, and 50 g of cyclohexanedimethanol, and a diacid mixture containing 71 g of adipic acid and 486 g of isophthalic acid. It heated up to 240 degreeC, stirring. Thereafter, a condensation reaction was performed for about 7-8 hours to obtain a thermosetting polyester resin having a hydroxyl value of 21, an acid value of 5, and a viscosity (Gardner) of Z-Z1.

실시예 2Example 2

2ℓ4구 플라스크에 온도계, 응축기, 교반기 및 콘덴서를 설치하고 승온장치를 부착하였다. 여기에 네오펜틸글리콜 223g, 1,6-헥산디올 59g, 에틸렌 글리콜 57g을 포함하는 글리콜 혼합물과 아디픽산 71g, 이소프탈릭산 131g 테레프탈릭산 355g을 포함하는 2가산 혼합물을 투입한 후 서서히 교반하면서 240℃로 승온하였다. 이후, 약 7 내지 8시간 동안 축합 반응을 수행하여 수산기값이 22, 산가가 4, 점도(가드너)가 V- 인 열경화성 폴리에스테르 수지를 수득하였다.A 2-liter four-necked flask was equipped with a thermometer, condenser, stirrer and condenser and a temperature raising device was attached. Here, a glycol mixture containing 223 g of neopentyl glycol, 59 g of 1,6-hexanediol, and 57 g of ethylene glycol was added thereto, and a diacid mixture containing 71 g of adipic acid and 355 g of isophthalic acid and 355 g of terephthalic acid was added thereto. It heated up as. Thereafter, a condensation reaction was performed for about 7 to 8 hours to obtain a thermosetting polyester resin having a hydroxyl value of 22, an acid value of 4, and a viscosity (Gardner) of V-.

실시예 3Example 3

2ℓ4구 플라스크에 온도계, 응축기, 교반기 및 콘덴서를 설치하고 승온장치를 부착하였다. 여기에 네오펜틸글리콜 244g, 에틸렌옥사이드가 2몰 부가된 당량이 169인 비스페놀 A 270g를 포함하는 글리콜 혼합물과 아디픽산 117g, 이소프탈릭산 166g, 테레프탈릭산 199g을 포함하는 2가산 혼합물을 투입한 후 서서히 교반하면서 240℃로 승온하였다. 약 7-8시간 동안 축합 반응을 수행하여 수산기값이 19, 산가가 1, 점도(가드너)가 V 인 열경화성 폴리에스테르 수지를 얻었다.A 2-liter four-necked flask was equipped with a thermometer, condenser, stirrer and condenser and a temperature raising device was attached. To this was added a glycol mixture containing 244 g of neopentyl glycol and 270 g of bisphenol A having an equivalent of 2 mol of ethylene oxide, and a diacid mixture containing 117 g of adipic acid, 166 g of isophthalic acid, and 199 g of terephthalic acid. It heated up to 240 degreeC, stirring. The condensation reaction was performed for about 7-8 hours to obtain a thermosetting polyester resin having a hydroxyl value of 19, an acid value of 1, and a viscosity (Gardner) of V.

실시예 4Example 4

2ℓ4구 플라스크에 온도계, 응축기, 교반기 및 콘덴서를 설치하고 승온장치를 부착하였다. 여기에 네오펜틸글리콜 257g, 메틸프로판디올 50g, 1,6-헥산디올 42g를 포함하는 글리콜 혼합물과 아디픽산 71g, 이소프탈릭산 240g, 테레프탈릭산 240g를 포함하는 2 가산 혼합물을 투입한 후 서서히 교반하면서 240℃로 승온하였다. 이후, 약 7-8시간 동안 축합 반응을 수행하여 수산기값이 21, 산가가 4, 점도(가드너)가 Z3인 열경화성 폴리에스테르 수지를 수득하였다.A 2-liter four-necked flask was equipped with a thermometer, condenser, stirrer and condenser and a temperature raising device was attached. Here, a glycol mixture containing 257 g of neopentyl glycol, 50 g of methyl propanediol, and 42 g of 1,6-hexanediol and a diacid mixture containing 71 g of adipic acid, 240 g of isophthalic acid, and 240 g of terephthalic acid were added thereto, and then slowly stirred. It heated up to 240 degreeC. Thereafter, a condensation reaction was performed for about 7-8 hours to obtain a thermosetting polyester resin having a hydroxyl value of 21, an acid value of 4, and a viscosity (Gardner) of Z3.

실시예 5Example 5

2ℓ4구 플라스크에 온도계, 응축기, 교반기 및 콘덴서를 설치하고 승온장치를 부착하였다. 여기에 네오펜틸글리콜 300g, 혼합된 사이클로헥산디메틸올 50g를 포함하는 글리콜 혼합물과 아디픽산 40g, 이소프탈릭산 480g를 포함하는 2 가산 혼합물을 첨가한 후 서서히 교반하면서 240℃로 승온하였다. 이후, 약 7-8시간 동안 축합 반응을 수행하여 수산기값이 19, 산가가 4, 점도(가드너)가 Z2인 열경화성 폴리에스테르 수지를 수득하였다.A 2-liter four-necked flask was equipped with a thermometer, condenser, stirrer and condenser and a temperature raising device was attached. A glycol mixture containing 300 g of neopentyl glycol and 50 g of mixed cyclohexanedimethylol and a diacid mixture containing 40 g of adipic acid and 480 g of isophthalic acid were added thereto, and then the temperature was raised to 240 ° C. while slowly stirring. Thereafter, a condensation reaction was performed for about 7-8 hours to obtain a thermosetting polyester resin having a hydroxyl value of 19, an acid value of 4, and a viscosity (Gardner) of Z2.

실시예 6Example 6

2ℓ4구 플라스크에 온도계, 응축기, 교반기 및 콘덴서를 설치하고 승온장치를 부착하였다. 여기에 네오펜틸글리콜 257g, 혼합된 사이클로헥산디메틸올 40g, 1,6-헥산디올 50g를 포함하는 글리콜 혼합물과 아디픽산 71g, 이소프탈릭산 240g, 테레프탈릭산 240g를 포함하는 2 가산 혼합물을 투입한 후 서서히 교반하면서 240℃로 승온하였다. 이후 약 7-8시간 동안 축합 반응을 수행하여 수산기 값이 21, 산가가 2, 점도(가드너)가 Z2인 열경화성 폴리에스테르 수지를 수득하였다.A 2-liter four-necked flask was equipped with a thermometer, condenser, stirrer and condenser and a temperature raising device was attached. Here, a glycol mixture containing 257 g of neopentyl glycol, 40 g of mixed cyclohexanedimethylol, and 50 g of 1,6-hexanediol and a diacid mixture containing 71 g of adipic acid, 240 g of isophthalic acid and 240 g of terephthalic acid were added thereto. It heated up to 240 degreeC, stirring slowly. Thereafter, a condensation reaction was performed for about 7-8 hours to obtain a thermosetting polyester resin having a hydroxyl value of 21, an acid value of 2, and a viscosity (Gardner) of Z2.

비교예 1Comparative Example 1

2ℓ4구 플라스크에 온도계, 응축기, 교반기 및 콘덴서를 설치하고 승온장치를 부착하였다. 여기에 네오펜틸글리콜 300g, 사이클로헥산디메틸올 50g를 포함하는 글리콜 혼합물과 아디픽산 40g, 이소프탈릭산 480g를 포함하는 2 가산 혼합물을 첨가한 후 서서히 교반하면서 240℃로 승온하였다. 이후, 약 7-8시간 동안 축합 반응을 수행하여 수산기값이 19, 산가가 4, 점도(가드너)가 Z인 열경화성 폴리에스테르 수지를 얻었다.A 2-liter four-necked flask was equipped with a thermometer, condenser, stirrer and condenser and a temperature raising device was attached. A glycol mixture containing 300 g of neopentyl glycol and 50 g of cyclohexanedimethylol was added thereto, and a diacid mixture containing 40 g of adipic acid and 480 g of isophthalic acid was added thereto, and the temperature was raised to 240 ° C. while gradually stirring. Thereafter, a condensation reaction was performed for about 7-8 hours to obtain a thermosetting polyester resin having a hydroxyl value of 19, an acid value of 4, and a viscosity (Gardner) of Z.

합성예 1~6 및 비교 합성예Synthesis Examples 1 to 6 and Comparative Synthesis Examples

상기 실시예 1 내지 6 및 비교예 1에서 각각 수득된 폴리에스테르 수지를 포함하는 PCM 하도용 도료의 도장의 특성을 알아보기 위하여 하기 표 1에 도시된 조성을 각각 적용하여 합성예 1 내지 6 및 비교 합성예1의 PCM 하도용 도료를 제조하였다. Synthesis Examples 1 to 6 and Comparative Synthesis by applying the compositions shown in Table 1, respectively, in order to find out the characteristics of the coating of the PCM paint for coating including the polyester resin obtained in Examples 1 to 6 and Comparative Example 1, respectively PCM paint coating material of Example 1 was prepared.

합성예 1Synthesis Example 1 합성예 2Synthesis Example 2 합성예 3Synthesis Example 3 합성예 4Synthesis Example 4 합성예 5Synthesis Example 5 합성예 6Synthesis Example 6 비교 합성예Comparative Synthesis Example 실시예(1)의 수지Resin of Example (1) 300(g)300 (g) 실시예(2)의 수지Resin of Example (2) 300(g)300 (g) 실시예(3)의 수지Resin of Example (3) 300(g)300 (g) 실시예(4)의 수지Resin of Example (4) 300(g)300 (g) 실시예(5)의 수지Resin of Example (5) 300(g)300 (g) 실시예(6)의 수지Resin of Example (6) 300(g)300 (g) 비교예(1)의 수지Resin of Comparative Example (1) 300(g)300 (g) 산화 티타늄(TiO2)Titanium Oxide (TiO 2 ) 100(g)100 g 100(g)100 g 100(g)100 g 100(g)100 g 100(g)100 g 100(g)100 g 100(g)100 g 크롬산 스트론늄Strontium chromium 100(g)100 g 100(g)100 g 100(g)100 g 100(g)100 g 100(g)100 g 100(g)100 g 100(g)100 g 분산제Dispersant 2(g)2 (g) 2(g)2 (g) 2(g)2 (g) 2(g)2 (g) 2(g)2 (g) 2(g)2 (g) 2(g)2 (g) 멜라민 경화제Melamine curing agent 30(g)30 (g) 30(g)30 (g) 30(g)30 (g) 30(g)30 (g) 30(g)30 (g) 30(g)30 (g) 30(g)30 (g) 산촉매Acid catalyst 3(g)3 (g) 3(g)3 (g) 3(g)3 (g) 3(g)3 (g) 3(g)3 (g) 3(g)3 (g) 3(g)3 (g) 소포제Antifoam 5(g)5 (g) 5(g)5 (g) 5(g)5 (g) 5(g)5 (g) 5(g)5 (g) 5(g)5 (g) 5(g)5 (g) 용제solvent 460(g)460 g 460(g)460 g 460(g)460 g 460(g)460 g 460(g)460 g 460(g)460 g 460(g)460 g system 1000(g)1000 g 1000(g)1000 g 1000(g)1000 g 1000(g)1000 g 1000(g)1000 g 1000(g)1000 g 1000(g)1000 g

멜라민 경화제로서는 사이멜-325(Cymel-325, Cytec industry제품)를 사용하였고, 용제로는 코코솔-100(K-100), 코코솔-150(K-150), 사이클로헥사논, 크실렌 및 셀로솔브 아세테이트의 혼합액을 사용하였다.As melamine curing agent, Cymel-325 (Cymel-325, manufactured by Cytec industry) was used, and as a solvent, Cocosol-100 (K-100), Cocosol-150 (K-150), cyclohexanone, xylene, and cello A mixed solution of sorb acetate was used.

폴리에스테르 수지를 포함하는 PCM 하도용 도료의 도막평가Coating Film Evaluation of PCM Undercoat Paint Containing Polyester Resin

표 1에 도시된 폴리에스테르 수지를 포함하는 도료의 특성을 알아보기 위해 상기 합성예 1 내지 6 및 비교 합성예에서 각각 제조된 하도용 도료를 소지에 도포하여 도막을 형성한 후 PCM 강판 상도 도료를 도장하여 도막의 특성을 평가하는 시험을 수행하였다. 그 결과를 표 2에 나타내었다.In order to examine the characteristics of the coating material comprising the polyester resin shown in Table 1, the coating material for each coat prepared in Synthesis Examples 1 to 6 and Comparative Synthesis Examples was applied to the substrate to form a coating film. The test was performed to evaluate the properties of the coating by coating. The results are shown in Table 2.

이때 사용되는 소지로는 인산아연 처리된 강판을 사용하였고 도막의 두께는 5±2㎛, 소지가 받는 표면온도는 240℃로 실시하였으며, 상도 도료로 수산기값이 0.5 내지 1% 이고, 분자량이 12,000이고, Tg가 30℃인 열경화성 수지를 사용하여 제조된 PCM 상도용 도료를 사용하였다.At this time, zinc phosphate-treated steel plate was used, and the thickness of the coating film was 5 ± 2㎛, and the surface temperature of the paper was 240 ℃. The top coating was a hydroxyl value of 0.5 to 1%, and a molecular weight of 12,000. , PCM coating material prepared using a thermosetting resin having a Tg of 30 ° C. was used.

합성예 1Synthesis Example 1 합성예 2Synthesis Example 2 합성예 3Synthesis Example 3 합성예 4Synthesis Example 4 합성예 5Synthesis Example 5 합성예 6Synthesis Example 6 비교 합성예Comparative Synthesis Example 광택(60 °)Polished (60 °) 9090 9191 9292 9090 9292 9292 9191 MEK 러빙MEK rubbing 100이상100 or more 100이상100 or more 100이상100 or more 100이상100 or more 100이상100 or more 100이상100 or more 100이상100 or more 가공성Machinability 2T2T 2T-2T- 2T-2T- 2T2T 3T3T 3T3T 2T2T 연필경도Pencil hardness FF FF 1H1H HH HH HH HH 부착성Adhesion 95/10095/100 95/10095/100 95/10095/100 90/10090/100 100/100100/100 100/100100/100 100/100100/100 내산성Acid resistance 양호Good 양호Good 양호Good 양호Good 양호Good 양호Good 양호Good 내알카리성Alkali resistance 양호Good 양호Good 양호Good 양호Good 양호Good 양호Good 양호Good 내습성Moisture resistance O O O O O 소지, 상도 밀착성Body, top adhesiveness O O O O

상기 표 2에서 소지 및 상도에 대한 밀착성을 표시하는 각 평가 항목은 다음과 같다. ◎ : 매우 양호, O: 양호, △: 보통, x: 불량을 의미한다.In Table 2, each evaluation item indicating the adhesion to the base and top coat is as follows. (Double-circle): Very good, O: Good, (triangle | delta): Normal, x: It means poor.

1. 광택 ; ASTM-D-523(미국재료시험협회규격(American Society for Testing and Materials)에서 정한 비금속 물질이 반사하는 광택을 측정하는 기준)에 의해 측정하였다.1. gloss; It was measured by ASTM-D-523 (a standard for measuring the gloss reflected by non-metallic materials determined by the American Society for Testing and Materials).

2. MEK Rubbing성 ; NCCA-II-18(National Coil Coaters Association에서 정한 용매 저항에 대한 평가 사양)에 의해 측정하였다.2. MEK Rubbing property; Measurement was made by NCCA-II-18 (evaluation specification for solvent resistance as determined by the National Coil Coaters Association).

3. 가공성 ; NCCA-II-19(National Coil Coaters Association에서 정한 "T" 밴드 시험법)에 의해 측정하였다.3. Machinability; Measurement was made by NCCA-II-19 ("T" band test method as defined by the National Coil Coaters Association).

4. 연필 경도 ; NCCA-II-12(National Coil Coaters Association에서 정한 상대적인 연필 경도 평가 사양)에 의해 측정하였다.4. pencil hardness; Measurement was made by NCCA-II-12 (relative pencil hardness evaluation specification set by the National Coil Coaters Association).

5. 부착성(C.E.T) ; NCCA-II-20(National Coil Coaters Association에서 정한 소지 부착성 시험법)에 의해 측정하였다.5. Adhesion (C.E.T); The measurement was carried out by NCCA-II-20 (Possessing adhesion test method as defined by the National Coil Coaters Association).

6. 내 산성 및 내 알칼리성 ; ASTM-D-1308(미국재료시험협회규격(American Society for Testing and Materials)에서 정한 유기물질의 마감재 상에 사용되는 가정용 화학약품에 대한 국제 기준)에 의해 측정하였다.6. Acid and alkali resistance; It was measured by ASTM-D-1308 (International Standard for Household Chemicals Used on Finishes of Organic Substances as defined by the American Society for Testing and Materials).

7. 내습성 ; 도막이 형성된 소지를 80℃ 끓는물에 침적시킨후, 변화된 도막의 상태를 20일 경과후 육안으로 판별함으로써 수행하였다.7. moisture resistance; After coating the formed film in 80 ℃ boiling water, it was performed by visually discriminating the state of the changed film after 20 days.

8. 소지 및 상도와의 밀착성 ; 동전을 이용하여 동일한 힘으로 도막을 눌러 긁어 줌으로써, 소지 및 상도로부터 도막이 떨어져 나가는 정도를 육안으로 판별하여 수행하였다.8. adhesion to body and top; By using a coin to scratch the coating film with the same force, it was performed by visually discriminating the degree of the coating film falling off the base and top coat.

표 2를 참조하면, 본 발명의 실시예들의 열경화성 폴리에스테르 수지를 포함하는 도료를 이용하여 형성된 도막은 비교 합성예의 도료로 제조된 도막에 대하여 전반전으로 동일한 특성을 나타내었다.Referring to Table 2, the coating film formed by using the coating material containing the thermosetting polyester resin of the embodiments of the present invention exhibited the same characteristics in the first half with respect to the coating film made of the coating material of Comparative Synthesis Example.

특히 혼합된 사이클로헥산디메틸올로 제조된 실시예 5 및 6의 열경화성 폴리에스테르 수지를 포함하는 합성예 5 및 6의 도료는 합성예 1 내지 4 및 비교 합성예 1의 도료보다 소지 및 상도와의 밀착성과 가공성이 우수한 특성을 갖음을 알 수 있다.In particular, the paints of Synthesis Examples 5 and 6 comprising the thermosetting polyester resins of Examples 5 and 6 made of mixed cyclohexanedimethylol had better adhesion to base materials and tops than those of Synthesis Examples 1 to 4 and Comparative Synthesis Example 1. It can be seen that the excellent workability and properties.

상술한 바와 같이 본 발명에 의하면 1,3-사이클로헥산디메탄올과 1,4-사이클로헥산디메탄올 혼합된 제1 글리콜과 제2 글리콜을 포함하는 글리콜 혼합물에 2가산 혼합물을 축합반응시키면 열경화성 폴리에스테르 수지를 제조할 수 있다.As described above, according to the present invention, a condensation reaction of a diacid mixture with a glycol mixture comprising a first glycol and a second glycol mixed with 1,3-cyclohexanedimethanol and 1,4-cyclohexanedimethanol results in thermosetting polyester. Resin can be manufactured.

상기한 방법으로 제조된 폴리에스테르 수지는 소지 및 상도에 대한 밀착성 및 도장후 가공성, 내습성이 우수한 PCM 하도용 도료를 제조할 수 있도록 적용된 다. 또한, 상기 열경화성 폴리에스테를 포함하는 PCM 하도용 도료는 우수한 기계적 물성 및 내화학적 물성을 유지하면서 용제와의 상용성을 높일 수 있어 안정적인 도막을 형성할 수 있다.The polyester resin prepared by the above method is applied to produce a PCM coating material for excellent adhesion to the base and top coat, workability after painting, moisture resistance. In addition, the PCM paint coating material containing the thermosetting polyester can increase the compatibility with the solvent while maintaining excellent mechanical and chemical properties can form a stable coating film.

상술한 바와 같이, 본 발명의 바람직한 실시예를 참조하여 설명하였지만 해당 기술 분야의 숙련된 당업자라면 하기의 특허 청구의 범위에 기재된 본 발명의 사상 및 영역으로부터 벗어나지 않는 범위 내에서 본 발명을 다양하게 수정 및 변경시킬 수 있음을 이해할 수 있을 것이다. As described above, although described with reference to a preferred embodiment of the present invention, those skilled in the art will be variously modified without departing from the spirit and scope of the invention described in the claims below. And can be changed.

Claims (14)

글리콜 총 당량에 대하여 1,3-사이클로헥산디메탄올과 1,4-사이클로헥산디메탄올 혼합된 제1 글리콜 5 내지 40%와 제2 글리콜 60 내지 95%를 포함하는 글리콜 혼합물; 및 아로마틱산, 알리파틱산 또는 이들의 혼합물을 포함하는 2가산 혼합물이 1.0: 1.0 내지 1.1 당량비로 축합된 PCM 도료용 폴리에스테르 수지.A glycol mixture comprising 5 to 40% of a first glycol and 60 to 95% of a second glycol mixed with 1,3-cyclohexanedimethanol and 1,4-cyclohexanedimethanol relative to the total equivalent glycol; And a diacid mixture comprising an aromatic acid, aliphatic acid or a mixture thereof in a polyester resin for PCM paint, wherein the diacid mixture is condensed at a ratio of 1.0: 1.0 to 1.1. 제1항에 있어서, 상기 제1 글리콜은 하기 화학식 (1)을 갖는 1,3-사이클로헥산디메탄올과 하기 화학식 (2) 1,4-사이클로헥산디메탄올이 1:1 비율로 혼합된 것을 특징으로 하는 PCM 도료용 폴리에스테르 수지.According to claim 1, wherein the first glycol is characterized in that 1,3-cyclohexanedimethanol having the formula (1) and the following formula (2) 1,4-cyclohexanedimethanol are mixed in a 1: 1 ratio Polyester resin for PCM coating to be.
Figure 112004061473368-PAT00003
------(1)
Figure 112004061473368-PAT00004
------(2)
Figure 112004061473368-PAT00003
------(One)
Figure 112004061473368-PAT00004
------(2)
제1항에 있어서, 상기 제2 글리콜은 사이클로헥산디메탄올, 에틸렌 글리콜, 프로필렌 글리콜, 메틸프로판디올, 네오펜틸 글리콜, 1,4-사이클로헥산디메틸올, 1,6-헥산디올, 에틸렌옥사이드 부가 비스페놀에이로 이루어진 군에서 선택된 적어도 하나를 포함하는 것을 특징으로 하는 PCM 도료용 폴리에스테르 수지.The method of claim 1, wherein the second glycol is cyclohexanedimethanol, ethylene glycol, propylene glycol, methylpropanediol, neopentyl glycol, 1,4-cyclohexanedimethylol, 1,6-hexanediol, ethylene oxide addition bisphenol Polyester resin for PCM paint, characterized in that it comprises at least one selected from the group consisting of a. 제1항에 있어서, 상기 아로마틱산은 프탈릭 안하이드라이드, 테트라하이드로 프탈릭 안하이드라이드, 이소프탈릭산, 테레프탈릭산로 이루어진 군에서 선택된 적어도 하나를 포함하는 것을 특징으로 하는 PCM 도료용 폴리에스테르 수지.The polyester resin of claim 1, wherein the aromatic acid comprises at least one selected from the group consisting of phthalic anhydride, tetrahydro phthalic anhydride, isophthalic acid and terephthalic acid. 제1항에 있어서, 상기 알리파틱산은 세바식산, 아디픽산 및 아젤라익산로 이루어진 군에서 선택된 적어도 하나를 포함하는 것을 특징으로 하는 PCM 도료용 폴리에스테르 수지.The polyester resin of claim 1, wherein the aliphatic acid comprises at least one selected from the group consisting of sebacic acid, adipic acid, and azelaic acid. 제1항에 있어서, 상기 아로마틱산은 상기 2가산 총당량의 50 내지 100%를 포함하고, 상기 알리파틱산은 상기 2가산 총당량의 0 내지 50%를 포함하는 것을 특징으로 하는 PCM 도료용 폴리에스테르 수지.The polyester resin of claim 1, wherein the aromatic acid comprises 50 to 100% of the total amount of diacids, and the aliphatic acid comprises 0 to 50% of the total amount of diacids. . 제1항에 있어서, 상기 PCM 도료용 폴리에스테르 수지는 하이드록시 값이 19 내지 21 이고, 산가가 5이하이고, 가드너 점도가 Z-Z3, 평균 분자량이 10,000 내지 35000인 것을 특징으로 하는 PCM 도료용 폴리에스테르 수지.The method of claim 1, wherein the polyester resin for PCM paint has a hydroxy value of 19 to 21, an acid value of 5 or less, Gardner viscosity of Z-Z3, the average molecular weight of 10,000 to 35000 for PCM paints Polyester resin. 글리콜 총 당량에 대하여 1,3-사이클로헥산디메탄올과 1,4-사이클로헥산디메탄올 혼합된 제1 글리콜 5 내지 40%와 제2 글리콜 60 내지 95%를 포함하는 글리콜 혼합물을 형성하는 단계;Forming a glycol mixture comprising 5-40% of a first glycol and 60-95% of a second glycol mixed with 1,3-cyclohexanedimethanol and 1,4-cyclohexanedimethanol relative to the total glycol equivalents; 아로마틱산, 알리파틱산 또는 이들의 혼합물을 포함하는 2가산 혼합물을 형 성하는 단계; 및Forming a diacid mixture comprising an aromatic acid, aliphatic acid or a mixture thereof; And 상기 글리콜 혼합물과 상기 2가산 혼합물을 1.0: 1.0 내지 1.1당량비로 축합 반응시켜 열경화성 폴리에스테르 수지를 형성하는 단계를 포함하는 PCM 도료용 폴리에스테르 수지 제조방법.Condensation reaction of the glycol mixture and the diacid mixture in a ratio of 1.0: 1.0 to 1.1 equivalents to form a thermosetting polyester resin polyester resin for PCM paint. 제8항에 있어서, 상기 제1 글리콜은 하기 화학식 (1)을 갖는 1,3-사이클로헥산디메탄올과 하기 화학식 (2) 1,4-사이클로헥산디메탄올이 1:1 비율로 혼합하여 형성하는 것을 특징으로 하는 PCM 도료용 폴리에스테르 수지 제조방법.The method of claim 8, wherein the first glycol is formed by mixing 1,3-cyclohexanedimethanol having the following formula (1) and 1,4-cyclohexanedimethanol of the following formula (2) in a 1: 1 ratio. Method for producing a polyester resin for PCM paint, characterized in that. 제8항에 있어서, 상기 제2 글리콜은 사이클로헥산디메탄올, 에틸렌 글리콜, 프로필렌 글리콜, 메틸프로판디올, 네오펜틸 글리콜, 1,4-사이클로헥산디메틸올, 1,6-헥산디올, 에틸렌옥사이드 부가 비스페놀에이로 이루어진 군에서 선택된 적어도 하나를 포함하는 것을 특징으로 하는 PCM 도료용 폴리에스테르 수지 제조방법.The method of claim 8, wherein the second glycol is cyclohexanedimethanol, ethylene glycol, propylene glycol, methylpropanediol, neopentyl glycol, 1,4-cyclohexanedimethylol, 1,6-hexanediol, ethylene oxide addition bisphenol Method for producing a polyester resin for PCM paint, characterized in that it comprises at least one selected from the group consisting of a. 제8항에 있어서, 상기 아로마틱산은 프탈릭 안하이드라이드, 테트라하이드로 프탈릭 안하이드라이드, 이소프탈릭산, 테레프탈릭산로 이루어진 군에서 선택된 적어도 하나를 포함하는 것을 특징으로 하는 PCM 도료용 폴리에스테르 수지 제조방법.The method of claim 8, wherein the aromatic acid is phthalic anhydride, tetrahydro phthalic anhydride, isophthalic acid, terephthalic acid, at least one selected from the group consisting of polyester resin for PCM paint production Way. 제8항에 있어서, 상기 알리파틱산은 세바식산, 아디픽산 및 아젤릭산로 이루 어진 군에서 선택된 적어도 하나를 포함하는 것을 특징으로 하는 PCM 도료용 폴리에스테르 수지 제조방법.The method of claim 8, wherein the aliphatic acid comprises at least one selected from the group consisting of sebacic acid, adipic acid, and azelic acid. 제8항에 있어서, 상기 아로마틱산은 상기 2가산 총당량의 50 내지 100%를 포함하고, 상기 알리파틱산은 상기 2가산 총당량 0 내지 50%를 포함하는 것을 특징으로 하는 PCM 도료용 폴리에스테르 수지 제조방법.The method of claim 8, wherein the aromatic acid comprises 50 to 100% of the total amount of diacids, the aliphatic acid comprises a polyester resin for PCM coating, characterized in that it comprises 0 to 50% of the total amount of diacids. Way. 제9항에 있어서, 상기 PCM 도료용 폴리에스테르 수지는 하이드록시 값이 19 내지 21 이고, 산가가 5이하이고, 가드너 점도가 Z-Z3, 평균 분자량이 10,000 내지 35000인 것을 특징으로 하는 PCM 도료용 폴리에스테르 수지 제조방법.The method of claim 9, wherein the polyester resin for PCM paint has a hydroxy value of 19 to 21, an acid value of 5 or less, Gardner viscosity of Z-Z3, the average molecular weight of 10,000 to 35000 for PCM paints Polyester resin manufacturing method.
KR1020040112688A 2004-12-27 2004-12-27 Pre coated metal coating polyester resin and method of preparing the same KR100644766B1 (en)