KR100669082B1 - Process for dyeing high functional synthetic fiber using vat dye - Google Patents

Process for dyeing high functional synthetic fiber using vat dye Download PDF

Info

Publication number
KR100669082B1
KR100669082B1 KR1020060083249A KR20060083249A KR100669082B1 KR 100669082 B1 KR100669082 B1 KR 100669082B1 KR 1020060083249 A KR1020060083249 A KR 1020060083249A KR 20060083249 A KR20060083249 A KR 20060083249A KR 100669082 B1 KR100669082 B1 KR 100669082B1
Authority
KR
South Korea
Prior art keywords
dyeing
dye
bat
vat
disperse
Prior art date
Application number
KR1020060083249A
Other languages
Korean (ko)
Inventor
전준형
김은철
이권선
김재환
Original Assignee
주식회사 삼광염직
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 주식회사 삼광염직 filed Critical 주식회사 삼광염직
Priority to KR1020060083249A priority Critical patent/KR100669082B1/en
Application granted granted Critical
Publication of KR100669082B1 publication Critical patent/KR100669082B1/en

Abstract

A method for dyeing a high functional synthetic fiber by using a vat dye is provided to enhance the friction, cleaning and daylight fastness. Vat dye for SP with the particle size of 0.01-0.25 micrometer is used. A closed type jet dyeing device is used in order to prevent the oxidation of the jet dye. The liquid ratio of dye is set as 1:5-20. Sodium hydrosulfite and sodium carbonate of 5-20 g/l are used as the reducing agents. The reduction injection temperature is 80-100 degrees in centigrade in order to increase the reducing effect. The sodium hydrosulfite is firstly injected and thereafter the sodium carbonate is injected in order to prevent the over-reduction.

Description

배트염료를 이용한 고기능성 합성섬유의 염색방법 {Process for dyeing high functional synthetic fiber using vat dye}Process for dyeing high functional synthetic fiber using vat dye

도 1은 배트염료 CIBANON OLIVE S-MD의 입도분석 실험결과를 도시한 것이다.Figure 1 shows the particle size analysis results of the bat dye CIBANON OLIVE S-MD.

도 2는 배트염료 CIBANON BROWN BR-MD의 입도분석 실험결과를 도시한 것이다.Figure 2 shows the particle size analysis results of the bat dye CIBANON BROWN BR-MD.

도 3은 배트염료 CIBANON BLACK B-01 MD의 입도분석 실험결과를 도시한 것이다.Figure 3 shows the particle size analysis results of the bat dye CIBANON BLACK B-01 MD.

도 4는 배트염료 CIBANON RED 2B MD의 입도분석 실험결과를 도시한 것이다.Figure 4 shows the particle size analysis results of the bat dye CIBANON RED 2B MD.

도 5는 배트염료 CIBANON GREEN B-MD의 입도분석 실험결과를 도시한 것이다.Figure 5 shows the particle size analysis test results of the bat dye CIBANON GREEN B-MD.

도 6은 배트염료 INDANTHREN BLUE C-R PLUS의 입도분석 실험결과를 도시한 것이다.Figure 6 shows the particle size analysis test results of the bat dye DANTANTREN BLUE C-R PLUS.

도 7은 배트염료 INDANTHREN BROWN C-BR PLUS의 입도분석 실험결과를 도시한 것이다.Figure 7 shows the results of the particle size analysis of the bat dye INDANTHREN BROWN C-BR PLUS.

도 8은 배트염료 INDANTHREN NAVY BLUE C-BL PLUS의 입도분석 실험결과를 도시한 것이다.Figure 8 shows the particle size analysis test results of the bat dye DANTANREN NAVY BLUE C-BL PLUS.

도 9는 배트염료 INDANTHREN DIRECT BLACK 5689의 입도분석 실험결과를 도시한 것이다.9 illustrates the results of particle size analysis of the bat dye DANT HREN DIRECT BLACK 5689.

도 10은 환원제 투입 온도변화별 조건 실험에서의 염색공정도이다.10 is a dyeing process in the experiment of the change of the reducing agent input temperature.

도 11은 환원제 투입 농도변화별 조건 실험에서의 염색공정도이다.11 is a dyeing process chart in the experiment of the conditions according to the concentration change of the reducing agent.

도 12, 13은 L/Pink Disperse, Vat 염색물 사진 비교Figures 12 and 13 compare L / Pink Disperse, Vat Dye Pictures

도 14, 15는 L/Red Disperse, Vat 염색물 사진 비교Figures 14 and 15 compare L / Red Disperse, Vat dye picture

도 16, 17은 Brown Disperse, Vat 염색물 사진 비교Figures 16 and 17 are Brown Disperse, Vat Dye Picture Comparison

도 18, 19는 Violet Disperse, Vat 염색물 사진 비교Figures 18 and 19 compare the Violet Disperse, Vat dye picture

도 20, 21은 Yellow Disperse, Vat 염색물 사진 비교20 and 21 is a Yellow Disperse, Vat Dye Pictures Comparison

본 발명은 합성섬유의 염색방법에 관한 것으로, 특히 자동차 시트커버, 침장용 및 건축용 원단과 같은 고부가가치 제품에 적용할 수 있는 배트염료를 이용한 고기능성 합성섬유의 염색방법에 관한 것이다.The present invention relates to a method for dyeing synthetic fibers, and more particularly, to a method for dyeing high-performance synthetic fibers using bat dyes that can be applied to high value-added products such as automobile seat covers, bedding and construction fabrics.

국내 섬유산업은 대표적인 수출주도형 산업 및 고용창출 산업으로 국가경제에 상당한 기여를 하였고, 국내 제조업에서 큰 비중을 차지하고 있는 산업이다.The domestic textile industry has contributed significantly to the national economy as a representative export-driven industry and job creation industry, and it is an industry that takes up a large portion of the domestic manufacturing industry.

21세기의 미래 섬유산업은 기존 소재를 사용한 시장규모는 점차 감소하고, 생활수준 향상 및 인간의 욕구변화에 대응하여 새로운 섬유소재가 수요를 주도하여 나갈 것으로 예상되며, 더 나아가 의류용 섬유보다는 자동차용 시트와 같은 산업용 섬유의 수요가 늘어날 것이라고 예상된다.In the future textile industry of the 21st century, the market size using existing materials will gradually decrease, and new textile materials will lead demand in response to the improvement of living standards and changes in human needs. The demand for industrial fibers such as sheets is expected to increase.

국내 합성섬유소재의 생산현황을 보면, 생산량의 80%가 PET(Polyethylene terephthalate) 섬유이고 10%가 나일론(Nylon), 그리고 기타 섬유들이 10% 정도로 PET의 생산량이 두드러지게 많고, 이러한 현상은 국내뿐만 아니라, 동남아시아 및 중국 등도 그러하다.According to the production status of domestic synthetic fiber materials, 80% of the production amount is PET (Polyethylene terephthalate) fiber, 10% is nylon (Nylon), and other fibers 10% of the production of PET, and this phenomenon is not only domestic Not so with Southeast Asia and China.

PET 섬유는 높은 강력, 낮은 흡습성, 열가소성, 내약품성이 우수하며, 특히 내열성이 있고 신장굴곡에 대하여 특유의 탄성을 지니고 있어 의류용으로는 제1의 합성섬유가 되었고, 의류용뿐만 아니라, 우수한 일광견뢰도를 요구하는 저융점사(LM fiber)를 중심으로 하는 침장용, 자동차용 및 건축용 등의 다양한 용도로 사용되고 있으며 더 많은 분야에 응용될 것이라 기대된다.PET fiber has high strength, low hygroscopicity, thermoplasticity and chemical resistance, especially heat resistance and unique elasticity against stretch bending, making it the first synthetic fiber for garments, as well as excellent daylight for clothing. It is used in various applications such as acupuncture, automobile, and construction centering on low melting point yarn (LM fiber) requiring fastness, and is expected to be applied to more fields.

PET 섬유의 염색은 주로 분산염료를 사용하여 고온고압의 상태로 염색하는 것이 일반적이고, PET를 분산염료로 염색할 때, 먼저 수중에 현탁해 있는 염료 미립자로부터 염료분자상태로 용해되고, 다음으로 염료분자가 섬유표면에 흡착되고, 마지막으로 섬유내부의 빈 공간으로 들어가서 확산되는 3단계 과정을 거쳐서 염색이 이루어진다.In general, the dyeing of PET fibers is performed by disperse dyes at high temperature and high pressure. When dyeing PETs with disperse dyes, the PET fibers are first dissolved in dye molecules from dye fine particles suspended in water, and then dyes. Molecules are adsorbed on the fiber surface, and finally dyeing occurs through a three-step process that enters and diffuses into the voids inside the fiber.

그러나, 분산염료를 사용하면 일광견뢰도가 좋지 못한 단점이 있고, 자동차 시트커버와 같은 고부가가치 제품은 우수한 일광견뢰도를 요구하기 때문에 일광견뢰도를 증진시키기 위한 염색공정 개발이 절실히 필요하다.However, the use of disperse dyes has a disadvantage in that the daylight fastness is not good, and high value-added products such as automobile seat covers require excellent daylight fastness, so it is urgently needed to develop a dyeing process to enhance the lightfastness.

또한, 고 일광견뢰도를 요구하는 분산염료는 가격이 비싸고 고온고압에서만 염색이 가능하기 때문에 에너지 소비가 많아지는 등의 이유로 생산원가가 높아진다. 따라서, 생산원가를 줄이고 고부가가치의 제품생산을 위해서는 좀 더 가격이 저렴한 염료로 대체하거나 이에 맞는 염색공정의 개발이 절실히 필요하다.In addition, since the dyes that require high daylight fastness are expensive and can be dyed only at high temperature and high pressure, the production cost is high due to the increased energy consumption. Therefore, in order to reduce production costs and produce high value-added products, it is urgently needed to replace dyes with lower cost or to develop dyeing processes suitable for them.

배트(VAT) 염료는 물에 불용성이고 섬유에 대한 친화성은 낮지만, 알칼리성 환원욕에서 환원시켜 얻어지는 수용성의 류코(leuco) 화합물이 섬유에 대하여 친화성을 갖기 때문에 염색할 때는 류코 화합물의 형태로서 섬유에 흡착시킨 후, 산화에 의하여 섬유상에서 원래의 불용성 염료로 복귀시키는 염료이며, 우수한 일광 및 세탁견뢰도를 얻을 수 있는 장점이 있다.VAT dyes are insoluble in water and have low affinity for fibers, but since the water-soluble leuco compounds obtained by reduction in alkaline reduction baths have affinity for fibers, they are fibers in the form of leuco compounds when dyed. After adsorbing on, it is a dye which returns to the original insoluble dye on a fiber by oxidation, and has an advantage of obtaining excellent daylight and washing fastness.

그러나, 배트염료로 염색하면 재현성이 떨어진다는 단점이 있기 때문에 주로 청바지(blue jean)와 같은 면 섬유의 염색에만 사용되고 있고, PET와 같은 합성섬유의 염색도 가능하지만 재현성을 나타내는데 큰 어려움이 있어 사용되지 않고 있는 실정이다.However, it is mainly used only for dyeing cotton fibers such as blue jean, and dyeing synthetic fibers such as PET is possible because of the disadvantage of poor reproducibility when dyeing with bat dye. I'm not doing it.

현재 배트염료를 사용하여 폴리에스테르 계열의 섬유를 염색하는 방법은 국내뿐만 아니라 세계 어떠한 나라에서도 없다.Currently, there is no method for dyeing polyester fiber using bat dye in any country in the world as well as in Korea.

PET, PTT(Polytrimethylene Terephthalate)와 같은 합성섬유를 고일광 분산염료 대신 비교적 가격이 저렴한 배트염료를 사용하여 염색한다면, 생산원가도 줄일 수 있을 뿐만 아니라, 우수한 마찰, 세탁 및 일광 등의 견뢰도를 확보할 수 있는 섬유제품을 생산할 수 있으므로, 자동차 시트 및 건축용 섬유와 같은 고부가가치 산업에 적용할 수 있을 것이라 기대된다.If synthetic fibers such as PET and Polytrimethylene Terephthalate (PTT) are dyed using relatively low cost bat dyes instead of high daylight dispersion dyes, production costs can be reduced, as well as excellent friction, washing and light fastness. It is expected that it can be applied to high value-added industries such as automobile seats and construction fibers as it can produce textile products.

따라서, 본 발명의 목적은 이전에 시도되지 않은 배트염료를 사용하여 PET와 같은 폴리에스테르 계열의 섬유를 염색하고, 배트염료의 취약점인 재현성을 높임과 동시에 일광, 세탁 및 마찰 등의 견뢰도를 증진시킬 수 있는 새로운 염색방법을 제 공하는 것이다.Accordingly, an object of the present invention is to dye polyester-based fibers such as PET, using bat dyes that have not been attempted before, and to improve reproducibility, which is a weak point of bat dyes, and to improve the fastness of daylight, washing, and friction. It is to provide a new method of dyeing.

본 발명의 다른 목적은 업체의 생산원가를 감소시키고 자동차 시트커버와 같은 고부가가치 제품에 적용할 수 있는 염색방법을 제공하는 것이다.Another object of the present invention is to reduce the production cost of the company and to provide a dyeing method that can be applied to high value-added products such as automobile seat cover.

본 발명은 상기한 목적을 달성하기 위하여, 폴리에스테르 계열 섬유를 염색함에 있어서, 고온안정성을 고려하여 염료의 입자크기 0.01 내지 0.25 ㎛의 SP(특별방법으로 강알칼리 상태에서 염색하는 방법)용 배트염료를 사용하고, 배트염료가 물이나 공기 중에서 산화되어 색상이 변하는 것을 방지하기 위해 밀폐형 제트 염색기를 사용하고, 재현성을 확보하기 위해 염색 액비를 1:5 내지 20으로 설정하고, 과환원을 막기 위해 환원제로서 Na2S2O4와 Na2CO3를 각각 5 내지 20 g/ℓ로 사용하고, 환원효과를 높이기 위해 환원제 투입온도를 80 내지 100℃로 하고, 과환원을 방지하기 위해 Na2S2O4를 먼저 투입한 후 Na2CO3를 투입하고, 배트염료에 적합하도록 분산제와 균염제를 0.1 내지 1 g/ℓ로 사용하고, 색상의 재현성을 확보하기 위해 염색 온도를 125 내지 130℃로 하고, 산화제로서 H2O2를 0.1 내지 1 g/ℓ로 사용하고, 산화공정을 125 내지 130℃에서 수행하는 것을 특징으로 하는 폴리에스테르 계열 섬유의 염색방법을 제공한다.
이하, 실시예를 들어 본 발명을 상세하게 설명한다.
In order to achieve the above object, the present invention, in dyeing polyester fiber, in consideration of high temperature stability of the dye (battery dyeing method in strong alkali state SP) of the particle size of 0.01 to 0.25 ㎛ of dyes Use a closed jet dyeing machine to prevent color change by oxidizing the bat dye in water or air, and set the dyeing liquid ratio to 1: 5 to 20 to ensure reproducibility, and as a reducing agent to prevent over-reduction. Na 2 S 2 O 4 and Na 2 CO 3 are used at 5 to 20 g / l, respectively, the reducing agent input temperature is 80 to 100 ° C. to increase the reducing effect, and Na 2 S 2 O to prevent over-reduction. 4 was added first, followed by Na 2 CO 3 , and dispersing and leveling agents were used at 0.1 to 1 g / l to suit the bat dye, and the dyeing temperature was 125 to 130 to ensure color reproducibility. It provides a dyeing method of polyester-based fibers, characterized in that it is set to ℃, H 2 O 2 as 0.1 to 1 g / L as the oxidizing agent, the oxidation process is carried out at 125 to 130 ℃.
Hereinafter, an Example is given and this invention is demonstrated in detail.

[실시예]EXAMPLE

1. 폴리에스테르 계열 섬유의 적합한 배트염료 선택1. Selection of suitable bat dyes for polyester fiber

폴리에스테르 계열 섬유의 적합한 배트염료를 선택하기 위해서 염료별 입도 분석실험을 하였으며, 그 결과는 도 1 내지 도 9에 도시된 바와 같다. 표 1은 배트염료의 일반적인 타입 특성을 나타낸 것이고, 표 2는 각 배트염료의 특성을 나타낸 것이다. 배트염료는 고온 안정성을 가져야 하므로 SP용 염료가 바람직하고, 분자크기가 분산염료와 동일하여야 하며, 크기의 분포가 일정해야 한다.In order to select a suitable bat dye of the polyester-based fiber, the particle size analysis was performed for each dye, and the results are shown in FIGS. 1 to 9. Table 1 shows the general type characteristics of the bat dye, Table 2 shows the characteristics of each bat dye. Since the bat dye should have high temperature stability, the dye for SP is preferable, the molecular size should be the same as the disperse dye, and the size distribution should be constant.

종류Kinds 최적 염색온도(℃)Optimal dyeing temperature (℃) 전해질 필요Electrolyte required 섬유친화도Fiber affinity IWIW 4545 OO 중간middle ININ 6060 XX 높음height IN SPIN SP 60 내지 8060 to 80 XX 높음height SPSP 8080 XX 주로 블랙 쉐이드(black shade)Mainly black shade

염료명Dye name CI NOCI NO 평균입자 크기(㎛)Average particle size (㎛) 특성characteristic CIBANON OLIVE S MDCIBANON OLIVE S MD -- 0.218 0.218 OLIVE, BROWN, 전형적인 카키류의 칼라염색에 좋다. 흡착율이 빠르고 군복염색에 좋음It is good for color dyeing of OLIVE, BROWN, typical khaki. Fast adsorption rate and good for military dyeing CIBANON BROWN BR MDCIBANON BROWN BR MD BR 01BR 01 0.3400.340 레벨링성이 좋기 때문에 가성소다를 절약하게 됨Good leveling properties save caustic soda CIBANON BLACK B-01 MDCIBANON BLACK B-01 MD -- 0.2960.296 칼라 자체가 블랙으로 나타나지는 않음(GREY용), 블랙칼라를 위해서는 콤비가 필요The color itself does not appear black (for GRAY), a combination is required for black color CIBA RED 2B MDCIBA RED 2B MD RE 10RE 10 0.3450.345 높은 온도에서 염착되고 최고의 콤비네이션 하기 좋은 염료이며 색의 변화가 점차적으로 일어남Dye at high temperatures, good dye for best combinations, gradually changing color CIBANON GREEN BF MDCIBANON GREEN BF MD -- 0.1760.176 레벨링성이 우수Excellent leveling CIBANON BLACK R-01 MDCIBANON BLACK R-01 MD -- -- 블랙의 토대 컬러(GREY용 X)Black base color (X for GRAY) INDANTHREN BLUE C-RS PLUSINDANTHREN BLUE C-RS PLUS BLUE 004BLUE 004 0.1350.135 -- INDANTHREN BROWN C-BR PLUSINDANTHREN BROWN C-BR PLUS BROWN 001BROWN 001 0.3320.332 -- INDANTHREN NAVY BLUE C-BL PLUSINDANTHREN NAVY BLUE C-BL PLUS -- 0.3550.355 -- INDANTHREN DIRECT BLACK 5589 PLUSINDANTHREN DIRECT BLACK 5589 PLUS -- 0.3720.372 --

2. 환원조건실험2. Reduction condition test

가. 환원제 투입 온도변화별end. Reductant Input Temperature Change

-실험목적: 적정 환원조건을 먼저 찾아 내기 위해 환원조제는 같은 DATA로 넣되, 조제 투입 온도를 달리하여 실험을 하였다(70, 80, 90℃).-Purpose of experiment: In order to find the proper reducing condition, the reducing aid was put into the same data, but the experiment was performed by changing the preparation input temperature (70, 80, 90 ℃).

-염료명: INDANTHREN BROWN C-BR PLUS 1%(OWF), INDANTHREN DIRECT BLACK 5578 1%(OWF)Dye name: INDANTHREN BROWN C-BR PLUS 1% (OWF), INDANTHREN DIRECT BLACK 5578 1% (OWF)

-시료명: P/P 160D 해도사(경사: 75/36 DTY, 위사: 130D 해도사, 30D 고신축사)-Sample name: P / P 160D sea island (Slope: 75/36 DTY, Weft: 130D sea island, 30D high stretch yarn)

-환원제: Na2S2O4(Hydrosufite) 10 g/ℓ, Na2CO3(소다회) 10 g/ℓ, 하이드로 주입후 1회 젓은 후, 소다회 투입(과환원을 막기 위해 알칼리를 하이드로 주입 이후에 투입).Reducing agent: Na 2 S 2 O 4 (Hydrosufite) 10 g / l, Na 2 CO 3 (soda ash) 10 g / l, stir once after hydro-injection, and then add soda ash (hydro injection of alkali to prevent over-reduction) Afterwards).

-염색온도: 120℃ × 30"Dyeing temperature: 120 ℃ × 30 "

-실험기기: 대림 스타릿 IR기(상하회전형)-Experimental equipment: Daelim Starlet IR (up and down rotation type)

-실험욕비: 1 : 10(100 ㎖)-Experiment bath ratio: 1: 10 (100 ml)

-염색공정: 도 10 참조.Dyeing process: see FIG.

-산화조건: H202(과산화수소) 35% 0.3 ㎖/ℓOxidation conditions: H 2 0 2 (hydrogen peroxide) 35% 0.3 ml / l

-산화방법: 70℃에서 냉각 후, 흐르는 찬물에 세척한 후, 다시 포트에 과산화수소를 넣고 찬물 100 ㎖를 채운 후, 다시 90℃로 승온한 후, 10분 레벨링을 주고 60℃로 바로 냉각.-Oxidation method: After cooling at 70 ° C, washed in running cold water, and then put hydrogen peroxide in the pot again, filled with 100 ml of cold water, and then heated up at 90 ° C, giving 10 minutes leveling and cooling directly to 60 ° C.

-가공방법: 산화처리 후, 흐르는 찬물에 세척한 후, 드라이온기에 약 1분 건조한 다음, 미니텐터에서 180℃로 1분간 4번씩 건조 후, 칼라 확인.Processing method: After oxidation treatment, washing in running cold water, drying for about 1 minute in a dry warmer, and then dried four times for 1 minute at 180 ℃ in a mini tenter, color check.

-실험결과: BROWN 염료는 환원온도나 산화처리에 많은 영향을 받지 않았고, RED염료의 경우는 환원온도나 산화처리 후에 많은 칼라변화가 있었다.-Experimental results: BROWN dye was not affected by reduction temperature or oxidation treatment, and RED dye had many color changes after reduction temperature or oxidation treatment.

먼저 환원온도는 90℃ 투입 시 가장 원래의 칼라에 가깝게 칼라가 올라왔으며, 환원시에는 Tenter에서 RED끼가 더욱더 살아나는 결과를 볼 수 있었다.First, the reduction temperature was raised to close to the original color when the 90 ℃ was added, and when the reduction was found that the RED meal in the Tenter more and more alive.

또한, 환원시 하이드로 투입 후, 소다회 투입 시 시료에 바로 투입하게 되면 과환원으로 인한 얼룩이 발생하여 환원제 투입시 주의가 요망된다.In addition, if the water is directly added to the sample after the addition of hydro when reducing, soda ash is generated due to over-reduced stains, care should be taken when the reducing agent is added.

나. 환원제 투입 농도 변화별I. Reducing agent input concentration change

-실험목적: 적정 염색조건을 찾아내기 위해 환원제 투입량을 달리하였으며, 산화제는 동일시 주고 산화온도를 달리하여 실험하였다.-Purpose of experiment: To find the proper dyeing condition, the input amount of reducing agent was changed, and the oxidizing agent was given the same and the experiment was carried out with different oxidation temperature.

-염료명: CIBANON RED 2B MD 5%(OWF)Dye name: CIBANON RED 2B MD 5% (OWF)

-시료명: P/P 160D 해도사(경사: 75/36 DTY, 위사: 130D 해도사, 30D 고신축사)-Sample name: P / P 160D sea island (Slope: 75/36 DTY, Weft: 130D sea island, 30D high stretch yarn)

-분산제, 균염제: 0.3 g/ℓDispersant, leveling agent: 0.3 g / l

-환원제: Na2S2O4(Hydrosufite) 10, 15, 20 g/ℓ, Na2CO3(소다회) 10, 15, 20 g/ℓ, 환원효과를 높이기 위해 90℃에서 솔루션으로 투입, 하이드로 주입 후, 소다회 투입(과환원을 방지).Reducing agent: Na 2 S 2 O 4 (Hydrosufite) 10, 15, 20 g / l, Na 2 CO 3 (soda ash) 10, 15, 20 g / l, added as a solution at 90 ° C to increase the reducing effect, hydro After injection, add soda ash (prevent overreduction).

-염색온도: 110 & 120℃ × 40"Dyeing temperature: 110 & 120 ℃ × 40 "

-실험기기: 대림 스타릿 IR기(상하회전형)-Experimental equipment: Daelim Starlet IR (up and down rotation type)

-실험욕비: 1 : 10(100 ㎖)-Experiment bath ratio: 1: 10 (100 ml)

-산화조건: H202(과산화수소) 35% 0.7 ㎖/ℓOxidation conditions: H 2 0 2 (hydrogen peroxide) 35% 0.7 ml / l

-산화방법: 70℃에서 냉각 후, 흐르는 찬물에 워싱한 후, 다시 포트에 과산화수소를 넣고 찬물 100 ㎖를 채운 후, 다시 130℃로 승온한 후, 10분 레벨링을 주고 70℃로 바로 냉각(도 11 참조).Oxidation method: After cooling at 70 ° C., wash in running cold water, add hydrogen peroxide to the pot, fill 100 ml of cold water, warm up again to 130 ° C., give 10 minutes leveling and cool directly to 70 ° C. (Fig. 11).

-가공방법: 산화처리 후, 흐르는 찬물에 세척한 후, 드라이온기에 약 1분 건조한 다음, 미니텐터에서 180℃로 2분간 건조 후, 칼라 확인.Processing method: After oxidation treatment, washing in running cold water, drying for about 1 minute in a dry warmer, and then drying for 2 minutes at 180 ℃ in a mini tenter, color check.

-실험결과: BROWN 염료는 환원온도나 산화처리에 많은 영향을 받지 않았고, RED 염료의 경우는 환원온도나 산화처리 후에 많은 칼라변화가 있었다.-Experimental results: BROWN dye was not affected by reduction temperature or oxidation treatment, and RED dye showed a lot of color change after reduction temperature or oxidation treatment.

환원온도는 90℃ 투입 시 가장 원래의 칼라에 가깝게 칼라가 올라왔으며 환원시에는 Tenter에서 RED끼가 더욱더 살아나는 결과를 볼 수 있었다.When the reduction temperature was 90 ℃, the color rose closer to the original color, and when it was reduced, the RED kittens were more alive in Tenter.

또한, 환원 시 하이드로 투입 후, 소다회 투입 시 시료에 바로 투입하게 되면 과환원으로 인한 얼룩이 발생하여 환원제 투입시 주의가 요망된다.In addition, if the water is directly added to the sample after the addition of hydro when reducing, soda ash is generated due to over-reduced stains, so care should be taken when the reducing agent is added.

3-1. 산화조건실험 Ⅰ3-1. Oxidation Condition Experiment Ⅰ

-실험방법: 적정 산화조건을 찾아내기 위해 산화제와 산화온도를 변화하여 실험-Experimental method: experiment by changing the oxidizer and oxidation temperature to find the proper oxidation condition

-염료명: CIBANON RED 2B MD 1%(OWF)Dye name: CIBANON RED 2B MD 1% (OWF)

-시료명 : P/P 160D 해도사(경: 75/36 DTY, 위: 130D 48F 해도사, 30D 24F 고수축)-Sample name: P / P 160D sea island (light: 75/36 DTY, above: 130D 48F sea island, 30D 24F high shrinkage)

-환원제 : Na2S2O4(Hydrosufite) 10 g/l, Na2CO3(소다회) : 10 g/l, 환원효과를 높이기 위해 90℃에서 솔루션으로 투입, 하이드로 주입 후, 소다회 투입-Reducing agent: Na 2 S 2 O 4 (Hydrosufite) 10 g / l, Na 2 CO 3 (soda ash): 10 g / l, added as a solution at 90 ℃ to increase the reducing effect, after hydro injection, soda ash

-염색온도 : 120℃ X 30"-Dyeing temperature: 120 ℃ X 30 "

-실험기기 : 고려 IR기(상하회전형)-Experimental equipment: Goryeo IR machine (up and down rotation type)

-실험욕비 : 1 : 10(토탈액비 100ml)-Experiment bath ratio: 1: 10 (Total solution ratio 100ml)

-산화조건 : H202(과산화수소) 35% 0.3ml/l, 0.6ml/l, 0.9ml/lOxidation Condition: H202 (Hydrogen Peroxide) 35% 0.3ml / l, 0.6ml / l, 0.9ml / l

-산화방법 : 70℃에서 냉각 후, 흐르는 찬물에 워싱한 후, 다시 포트에 과산화수소를 넣고, 찬물 100ml를 채운 후, 다시 90℃, 110℃, 120℃로 승온한 후, 10분 레벨링을 주고 60℃로 바로 냉각.-Oxidation Method: After cooling at 70 ℃, wash in running cold water, put hydrogen peroxide in the pot again, fill with 100ml of cold water, raise the temperature to 90 ℃, 110 ℃, 120 ℃ again, give 10 minutes leveling Cool directly to ℃.

-가공방법 : 산화처리 후, 흐르는 찬물에 워싱한 후, 드라이온기에 약 1분 건조한 다음, 미니텐터에서 180℃로 1분간 4번씩 건조 후, 칼라 확인.-Processing method: After oxidation treatment, wash in running cold water, dry for about 1 minute in a dry warmer, and then dry 4 times for 1 minute at 180 ℃ in a mini tenter, and then check the color.

-실험결과: 120℃ 텐터 가공시 과수 0.3ml와 0.6ml의 color는 비슷한데 0.9ml를 넣은 것은 redish함,-Experimental results: 0.3ml and 0.6ml of fruit are similar in the tenter processing at 120 ℃ but 0.9ml is redish,

120℃ 건조시 3ml과 6ml을 사용한것 보다 9ml를 사용하는 것이 redish. 같은 온도를 기준으로 산화제를 많이 쓰면 redish 해짐, 같은 산화제를 기준으로 온도가 높을수록 redish, 재연성이 높아짐.It is redish to use 9ml rather than 3ml and 6ml when drying at 120 ℃. If you use more oxidant based on the same temperature, it becomes redish. The higher the temperature based on the same oxidant, the more redish and recombustible.

3-2. 산화조건실험 II3-2. Oxidation Condition Test II

-실험방법 : 적정산화조건을 찾아내기 위해 산화조제와 산화온도를 달리하여 실험-Experimental Method: Experiment with different oxidation aid and oxidation temperature to find proper oxidation condition

-염료명 : CIBANON RED 2B MD : 1%(OWF)Dye Name: CIBANON RED 2B MD: 1% (OWF)

-시료명 : P/P 160D 해도사(경: 75/36 DTY, 위: 130D 48F)Sample name: P / P 160D sea island (light: 75/36 DTY, upper: 130D 48F)

-환원제 : Na2S2O4(Hydrosufite) : 10 g/l, Na2CO3(소다회) : 10 g/l, 환원효과를 높이기 위해 90℃에서 솔루션으로 투입Reducing agent: Na2S2O4 (Hydrosufite): 10 g / l, Na2CO3 (soda ash): 10 g / l, added as a solution at 90 ℃ to increase the reducing effect

-염색온도 : 120℃ X 30"-Dyeing temperature: 120 ℃ X 30 "

-실험기기 : 고려 IR기(상하회전형)-Experimental equipment: Goryeo IR machine (up and down rotation type)

-실험욕비 : 1 : 10(토탈액비 100ml)-Experiment bath ratio: 1: 10 (Total solution ratio 100ml)

-산화조건 : H202(과산화수소) 35% 0.6ml/l, 0.7ml/l, 0.8ml/l-Oxidation Condition: H202 (Hydrogen Peroxide) 35% 0.6ml / l, 0.7ml / l, 0.8ml / l

-산화방법 : 70℃에서 냉각 후, 흐르는 찬물에 워싱한 후, 다시 포트에 과산화수소를 넣고 찬물 100ml를 채운 후, 다시 120℃, 125℃, 130℃로 승온한 후, 10 분 레벨링을 주고 70℃로 바로 냉각함.-Oxidation method: After cooling at 70 ℃, wash in running cold water, put hydrogen peroxide in the pot again and fill with 100ml of cold water, then warm up to 120 ℃, 125 ℃, 130 ℃, give 10 minutes leveling and 70 ℃ Cool directly to.

-실험결과: 120℃ 산화 : 가공 후, color 상태 대체적으로 유사. 과산화수소 8ml/l를 사용시 yellowish 해짐,-Experimental Results: 120 ℃ Oxidation: After processing, color status is generally similar. Yellowish when 8 ml / l of hydrogen peroxide is used,

125℃ 산화 : 가공 후, color 상태 유사(과수 6.7.8ml/l) 가공, 건조상태 거의 유사.125 ℃ Oxidation: Similar to color after processing (Fruit 6.7.8ml / l), almost similar to dry state.

130℃ 산화 : 가공 후, color 상태 유사(과수 6.7.8ml/l) 가공, 건조상태 거의 유사.130 ℃ Oxidation: Similar to color after processing (Fruit 6.7.8ml / l), almost similar to dry state.

4. 최적염색조건실험4. Optimal dyeing condition test

○ 염료명 : CIBANON RED 2B MD : 5%(OWF)○ Dye Name: CIBANON RED 2B MD: 5% (OWF)

○ 시료명 : P/P 160D 해도사(경: 75/36 DTY, 위: 130D 48F 해도사) 분산제, 균염제 : 0.3g/l○ Sample name: P / P 160D seaweed yarn (light: 75/36 DTY, above: 130D 48F seaweed yarn) Dispersant, leveling agent: 0.3g / l

○ 환원제 : Na2S2O4(Hydrosufite) : 10, 15, 20g/l, Na2CO3(소다회) : 10, 15, 20g/l ○ Reducing agent: Na2S2O4 (Hydrosufite): 10, 15, 20g / l, Na2CO3 (soda ash): 10, 15, 20g / l

○ 염색온도 : 120(125)℃ X 40"○ Dyeing temperature: 120 (125) ℃ X 40 "

○ 실험기기 : 고려 IR기(상하회전형)○ Laboratory equipment: Goryeo IR machine (up and down rotation type)

○ 실험욕비 : 1 : 10(토탈액비 100ml)○ Experiment bath ratio: 1: 10 (Total solution ratio 100ml)

○ 실험방법 : 적정 염색조건을 찾아내기 위해 환원조제, 산화조제는 동일시 주고 염료 DATA와 산화온도를 달리하여 실험 .○ Experimental method: To find the proper dyeing condition, the reducing and oxidizing agents should be identified and the dye data and the oxidation temperature should be changed.

○ 산화조건 : H202(과산화수소) 35%, 0.7ml/l○ Oxidation conditions: H202 (Hydrogen peroxide) 35%, 0.7ml / l

○ 산화방법 : 70℃에서 냉각 후, 흐르는 찬물에 워싱한 후, 다시 포트에 과산화수소를 넣고 찬물 100ml를 채운 후, 다시 130℃ 로 승온한 후, 10분 레벨링을 주고 70℃로 바로 냉각.○ Oxidation method: After cooling at 70 ℃, wash in running cold water, put hydrogen peroxide in the pot again, fill with 100ml of cold water, raise the temperature to 130 ℃ again, give 10 minutes leveling and cool directly to 70 ℃.

○ 가공방법 : 산화처리 후, 흐르는 찬물에 워싱한 후, 드라이온기에 약 1분 건조한 다음 미니텐터에서 180℃로 2분간 건조 후, 칼라 확인.○ Processing method: After oxidation treatment, wash in running cold water, and then dry for about 1 minute in dry warmer, and then dry for 2 minutes at 180 ℃ in mini tenter, check color.

○ 실험결과○ Experimental results

- 환원제 적정 사용량 확립-Establish proper amount of reducing agent

- 환원제 사용량에 따른 Na2CO3(소다회) 사용량 확립-Establishment of Na2CO3 (soda ash) usage according to reducing agent usage

- 염색온도 확립-Establishment of dyeing temperature

- 산화제 사용량 및 공정온도 확립-Oxidizer usage and process temperature

5. Direct Black DB 염료의 최적염색조건 실험5. Experimental Optimal Dyeing Condition for Direct Black DB Dye

○ 염료명 : Direct Black DB : 1%(OWF)○ Dye Name: Direct Black DB: 1% (OWF)

○ 시료명 : P/P 160D 해도사(경: 75/36 DTY, 위: 130D 48F 해도사), 분산제, 균염제 : 0.3g/l○ Sample Name: P / P 160D Sea Island Yarn (Light: 75/36 DTY, Above: 130D 48F Sea Island Yarn), Dispersant, Leveling Agent: 0.3g / l

○ 환원제 : Na2S2O4(Hydrosufite) : 10 g/l, Na2CO3(소다회) : 10 g/l ○ Reducing agent: Na2S2O4 (Hydrosufite): 10 g / l, Na2CO3 (soda ash): 10 g / l

○ 염색온도 : 120℃ X 40"○ Dyeing temperature: 120 ℃ X 40 "

○ 실험기기 : 고려 IR기(상하회전형)○ Laboratory equipment: Goryeo IR machine (up and down rotation type)

○ 실험욕비 : 1 : 10(토탈액비 100ml)○ Experiment bath ratio: 1: 10 (Total solution ratio 100ml)

○ 실험방법 : 적정염색조건을 찾아내기위해 환원조제, 산화조제는 동일시 주고 염료 DATA와 산화온도를 달리하여 실험함○ Experimental method: To find the proper dyeing condition, the reducing and oxidizing agents should be identified and tested by different dye data and oxidation temperature.

○ 산화조건 : H202(과산화수소) 35% 0.7ml/l○ Oxidation conditions: H202 (Hydrogen peroxide) 35% 0.7ml / l

○ 산화방법 : 70℃에서 냉각 후, 흐르는 찬물에 워싱한 후, 다시 포트에 과산화수소를 넣고 찬물 100ml를 채운 후, 다시 130℃로 승온한 후, 10분 레벨링을 주고 70℃로 바로 냉각함.○ Oxidation method: After cooling at 70 ℃, wash in running cold water, put hydrogen peroxide in the pot again, fill with 100ml of cold water, raise the temperature to 130 ℃ again, give 10 minutes leveling and cool immediately to 70 ℃.

○ 실험결과○ Experimental results

- 다른 염료와 동일하게 실험 결과가 나왔음-Experimental results came out like other dyes

- 따라서 아래와 같은 염료로 0.01%, 0.05%, 0.1%, 0.2%, 0.5%, 1.0%, 2.0%, 5.0% 최적염색실험을 하였음.
YELLOW GCN PINK R BLUE BC BROWN BR OLIVE T VIOLET 2R ORANGE 2RT GREEN FBB OLIVE MW
-The following dyes were used for 0.01%, 0.05%, 0.1%, 0.2%, 0.5%, 1.0%, 2.0% and 5.0% optimal dyeing experiments.
YELLOW GCN PINK R BLUE BC BROWN BR OLIVE T VIOLET 2R ORANGE 2RT GREEN FBB OLIVE MW

삭제delete

도 12 내지 도 21은 각 색상별로 분산염료와 배트염료를 이용하여 염색한 염색물 사진을 비교한 것으로, 배트염료 염색물의 품질이 분사염료 염색물에 비하여 동등 이상 우수함을 확인할 수 있다.12 to 21 is a comparison of the dyeing the dyeing using the dyes and the dye dye for each color, it can be confirmed that the quality of the bat dye dyes are equal or better than the spray dye dyes.

6. 염색 견뢰도 테스트
1) L/Pink Disperse, Vat염료 견뢰도 결과
Acetate Cotton Nylon PET Acrylic Wool 변퇴색 물견뢰도 Disperse 5 5 4-5 4-5 5 54-5 Vat 5 5 5 5 5 54-5 세탁견뢰도 Disperse 5 5 5 5 5 54-5 Vat 5 5 5 5 5 54-5 습마찰견뢰도 일광 견뢰도 20 시간 Disperse Vat 40 시간 Disperse Vat 승화견뢰도 Disperse Vat
6. Dyeing color fastness test
1) L / Pink Disperse, Vat Dye Fastness Result
Acetate Cotton Nylon PET Acrylic Wool Fading Water fastness Disperse 5 5 4-5 4-5 5 54-5 Vat 5 5 5 5 5 54-5 Color fastness Disperse 5 5 5 5 5 54-5 Vat 5 5 5 5 5 54-5 Wet Friction Fastness Daylight fastness 20 hours Disperse Vat 40 hours Disperse Vat Sublimation fastness Disperse Vat

삭제delete

2) L/Red Disperse, Vat염료 견뢰도 결과
Acetate Cotton Nylon PET Acrylic Wool 변퇴색 물견뢰도 Disperse 5 5 5 5 5 54-5 Vat 5 5 4-5 5 5 4-54-5 세탁견뢰도 Disperse 5 5 5 5 5 54-5 Vat 4-5 4-5 4 4-5 5 54-5 습마찰견뢰도 일광 견뢰도 20 시간 Disperse Vat 40 시간 Disperse Vat 승화견뢰도 Disperse Vat
2) L / Red Disperse, Vat dye fastness results
Acetate Cotton Nylon PET Acrylic Wool Fading Water fastness Disperse 5 5 5 5 5 54-5 Vat 5 5 4-5 5 5 4-54-5 Color fastness Disperse 5 5 5 5 5 54-5 Vat 4-5 4-5 4 4-5 5 54-5 Wet Friction Fastness Daylight fastness 20 hours Disperse Vat 40 hours Disperse Vat Sublimation fastness Disperse Vat

삭제delete

3) Brown Disperse, Vat염료 견뢰도 결과
Acetate Cotton Nylon PET Acrylic Wool 변퇴색 물견뢰도 Disperse 5 5 4-5 5 5 54-5 Vat 5 5 4-5 5 5 54-5 세탁견뢰도 Disperse 5 5 4-5 5 5 54-5 Vat 5 5 4-5 5 5 54-5 습마찰견뢰도 일광 견뢰도 20 시간 Disperse Vat 40 시간 Disperse Vat 승화견뢰도 Disperse Vat
3) Brown Disperse, Vat Dye Fastness Result
Acetate Cotton Nylon PET Acrylic Wool Fading Water fastness Disperse 5 5 4-5 5 5 54-5 Vat 5 5 4-5 5 5 54-5 Color fastness Disperse 5 5 4-5 5 5 54-5 Vat 5 5 4-5 5 5 54-5 Wet Friction Fastness Daylight fastness 20 hours Disperse Vat 40 hours Disperse Vat Sublimation fastness Disperse Vat

삭제delete

4) Violet Disperse, Vat염료 견뢰도 결과
Acetate Cotton Nylon PET Acrylic Wool 변퇴색 물견뢰도 Disperse 5 5 5 5 5 54-5 Vat 5 5 5 5 5 54-5 세탁견뢰도 Disperse 5 5 5 5 5 54-5 Vat 4 4-5 2 4 4-5 44-5 습마찰견뢰도 일광 견뢰도 20 시간 Disperse Vat 40 시간 Disperse Vat 승화견뢰도 Disperse Vat
4) Violet Disperse, Vat Dye Fastness Result
Acetate Cotton Nylon PET Acrylic Wool Fading Water fastness Disperse 5 5 5 5 5 54-5 Vat 5 5 5 5 5 54-5 Color fastness Disperse 5 5 5 5 5 54-5 Vat 4 4-5 2 4 4-5 44-5 Wet Friction Fastness Daylight fastness 20 hours Disperse Vat 40 hours Disperse Vat Sublimation fastness Disperse Vat

삭제delete

5) Yellow Disperse, Vat염료 견뢰도 결과
Acetate Cotton Nylon PET Acrylic Wool 변퇴색 물견뢰도 Disperse 5 5 4-5 5 5 4-54-5 Vat 5 5 5 5 5 54-5 세탁견뢰도 Disperse 5 5 4-5 5 5 4-54-5 Vat 5 5 5 5 5 54-5 습마찰견뢰도 일광 견뢰도 20 시간 Disperse Vat 40 시간 Disperse Vat 승화견뢰도 Disperse Vat
5) Yellow Disperse, Vat Dye Fastness Result
Acetate Cotton Nylon PET Acrylic Wool Fading Water fastness Disperse 5 5 4-5 5 5 4-54-5 Vat 5 5 5 5 5 54-5 Color fastness Disperse 5 5 4-5 5 5 4-54-5 Vat 5 5 5 5 5 54-5 Wet Friction Fastness Daylight fastness 20 hours Disperse Vat 40 hours Disperse Vat Sublimation fastness Disperse Vat

삭제delete

표 9는 상술한 테스트 결과를 토대로 배트염료를 이용한 PET 염색의 최적 염색공정을 요약한 것이다.
Factor 최적 특 징 염료 Type SP용 염료 - - 고온 안정성을 가져야함 분자 크기 0.25㎛ 이내 - - 분자 크기가 분산염료와 동일하여야 하며 크기의 분포가 일정 해야 함 염색기 JET 염색기 밀폐형 - VAT염료가 물이나 공기중에서 산화되 어 Color가 변화 하기 때문에 밀폐형 추천함 염색 액비 1:10 - 실험실과 현장과의 재현성 확보 환원제 Na2S2O4 10g/l - 염색시 온도가 고온으로 올라가기 때문에 과 환원을 막기 위해서 환원제 사용량을 적게 사용함 Na2CO3 10g/l - 일반적으로 NaOH를 사용하나 염색 시 온도가 고온으로 올라가기 때문에 과 환원을 막기 위해서 환원제 사용량을 적게 사용함 환원제 투입 온도 - 90℃ - 환원효과를 높이기 위함(과 환원방지) Na2S2O4 먼저 투입 후 Na2CO3 투입 분산제 - 0.3g/l - VAT 염료에 적합한 분산제 선택 (조제 회사와 공동개발 하였음) 균염제 - 0.3g/l - VAT 염료에 적합한 균염제 선택 (조제 회사와 공동개발 하였음) 염색 온도 125~130℃ × 40min - 120℃ 이상에서 Color의 재현성이 양호함 산화제 H2O2 0.7g/l - 산화제 사용량이 증가하여도 Color 변화가 없음 산화 공정 125~130℃ × 20min - 산화 시간을 더 주어도 Color 변화가 없음
Table 9 summarizes the optimal dyeing process of PET dyeing using bat dye based on the above test results.
Factor optimal Characteristic Dye Type Dye for SP - -Must have high temperature stability Molecular size Within 0.25㎛ - -The molecular size must be the same as the disperse dye and the size distribution must be constant Dyeing Machine JET Dyeing Machine Hermetic -Closed type is recommended because VAT dye is oxidized in water or air to change color. Dyeing liquid 1:10 -Reproducibility between the laboratory and the field reducing agent Na2S2O4 10 g / l -Since dyeing temperature rises to high temperature, less amount of reducing agent is used to prevent over reduction. Na2CO3 10 g / l -In general, NaOH is used, but the amount of reducing agent used is small to prevent over reduction because the temperature rises to high temperature during dyeing. Reductant input temperature - 90 ℃ -To increase the reduction effect (prevent reduction), add Na2S2O4 first and then Na2CO3 Dispersant - 0.3g / l -Selection of dispersant suitable for VAT dyes (co-development with formulation company) Leveling agent - 0.3g / l -Selecting suitable leveling agent for VAT dye (co-development with preparation company) Dyeing temperature 125 ~ 130 ℃ × 40min -Color reproducibility is good above 120 ℃ Oxidant H2O2 0.7g / l -No change in color even when the amount of oxidant is increased Oxidation process 125 ~ 130 ℃ × 20min -No change in color even after giving more oxidation time

삭제delete

우리나라는 세계에서 현재 자동차 수출 3위 국가인 만큼 이에 관련된 기술개발이 절실히 요구되고 있으며, 고급 자동차용 시트커버는 수입되고 있는 실정이어서 본 발명의 개발로 수입대체 효과를 볼 수 있으며, 또한 고급 자동차 시트커버용 원단을 수출할 수 있는 계기를 마련할 수 있고, 이종 업종인 자동차 산업을 한 단계 업그레이드시킬 수 있는 계기를 마련할 수 있다.As Korea is currently the world's third-largest automobile exporter in the world, there is an urgent need for technological development, and high-end automobile seat covers are being imported. It is possible to prepare an opportunity to export cover fabrics and to upgrade the automobile industry, which is a heterogeneous industry.

또한, 섬유시장의 편성물시장 중심 기술 용도전개 부분에서도 본 발명의 편성물 제품에 대한 염색 가공기술 확보로 기술적인 우위를 얻을 수 있다.In addition, it is possible to obtain a technical superiority by securing the dyeing processing technology for the knitted product of the present invention in the knitted product market-oriented technology development part of the textile market.

본 발명에 따른 파급효과의 기술적인 면을 살펴보면, 현재 PET 소재 관련 기술은 PET 고분자 중합기술, PET 원사 제조기술 확립된 상태이며, 전처리, 염색가공기술 등의 기초 상품화 기술개발 또한, 확립단계에 들어서 있다.Looking at the technical aspects of the ripple effect according to the present invention, the current PET material-related technology is the PET polymer polymerization technology, PET yarn manufacturing technology established state, the development of basic commercialization technology such as pretreatment, dyeing processing technology, etc. have.

PTT 섬유가 국내에 뿌리를 내리기 위해서는 적합한 용도개발을 통한 최종상품으로의 응용 기술개발이 중요하다.In order for PTT fiber to take root in Korea, it is important to develop application technology as a final product through proper use development.

그러기 위해서는 섬유산업의 꽃이라 할 수 있는 염색산업에서 소비자들의 다양한 욕구를 충족시킬 수 있는 기술 개발이 절실히 필요한 시점이다.To this end, it is time to develop technology that can satisfy various needs of consumers in the dyeing industry, which is the flower of the textile industry.

본 발명의 결과로 고일광, 세탁, 마찰견뢰도를 요구하는 섬유제품에서 선진국과 동등한 상태에서의 최종제품의 시장 및 기술 우의를 차지할 수 있는 염색공정기술 및 상품화 기술을 확립할 수 있다.As a result of the present invention, it is possible to establish a dyeing process technology and a commercialization technology that can occupy the market and technical advantages of the final product in the state equivalent to developed countries in textile products requiring high daylight, washing and friction fastness.

자동차 Seat cover, 침장용 및 건축용의 소재로 사용되기 위해서는 원사의 고유 물성뿐만 아니라, 염색 및 가공 원부재료의 선별과 적용기술 매우 절실히 필요로 하고 있다.In order to be used as a material for automobile seat cover, bedding and construction, not only the inherent properties of yarn, but also the selection and application technology of dyeing and processing raw materials are very much needed.

따라서 본 발명의 결과 자동차 Seat cover, 침장용 및 건축용 섬유소재의 산업용도로의 확대 전개에 필요한 기술 개발 확보가 가능하다.Therefore, as a result of the present invention it is possible to secure the development of technology necessary for the expansion and development of automobile seat cover, bedding and building textile materials for industrial roads.

본 발명에 따른 경제산업적인 측면을 살펴보면,Looking at the economic and industrial aspects of the present invention,

우리나라는 세계에서 현재 자동차 수출 3위 국가인 만큼 이에 관련된 기술개발이 절실히 요구되고 있으며, 고급 자동차용 Seat cover는 전량 수입되고 있는 실정이나, 본 발명으로 수입대체 효과를 볼 수 있으며,As Korea is currently the world's third-largest automobile exporter in the world, there is an urgent need for technological development.

또한 고급 자동차용 Seat cover용 원단을 수출할 수 있는 계기를 마련할 수 있다.In addition, it is possible to prepare an opportunity to export fabrics for high-end automotive seat covers.

특히, 향후에 신섬유 소재의 상품전개가 활발히 될 경우,In particular, when new product development of new fiber material becomes active in the future,

대부분 중소기업형인 Down Stream 업체에 대한 기술지원/보급 System이 구축하여 Polyester계 섬유소재의 고부가 제품생산을 위한 국내 Network System of Technical Research & Development 확보로 기술의 공유가 가능할 것으로 판단된다.Most of the technology support / distribution system for Downstream companies, which are small and medium-sized companies, will be established, and technology sharing will be possible by securing domestic network system of technical research & development for high value-added products of polyester fiber materials.

섬유시장의 편성물시장 중심 기술 용도전개 부분에서도 본 발명의 편성물제품에 대한 염색 가공기술 확보로 기술적인 우위가 확실할 것으로 생각된다.Even in the development of application of technology centered on the knitted fabric market of the textile market, it is believed that the technical superiority is assured by securing the dyeing processing technology for the knitted product of the present invention.

본 발명의 활용방안으로는 향상된 견뢰도의 Polyester계 섬유소재를 이용하여 다양한 최종제품을 개발할 수 있으며,As a method of utilizing the present invention, it is possible to develop a variety of final products by using a polyester fiber material of improved fastness,

비의류용도인 자동차 Seat cover, 침장용 및 건축용 원단을 염색하는 업체에서Companies dyeing automotive seat covers, bedding and construction fabrics for non-clothing purposes

본 발명을 적용시켜 경쟁력 있는 제품을 생산할 수 있는 효과를 제공 받을 수 있다.By applying the present invention can be provided with the effect of producing a competitive product.

Claims (11)

배트염료를 이용하여 폴리에스테르 계열 섬유를 염색하며,Dyeing polyester fiber using bat dye, 염료의 입자크기 0.01 내지 0.25 ㎛의 SP(특별방법으로 강알칼리 상태에서 염색하는 방법)용 배트염료를 사용하는 것을 특징으로 하는 배트염료를 이용한 고기능성 합성섬유의 염색방법.Dyeing method of high-performance synthetic fibers using a bat dye, characterized in that the bat dye for SP (method of dyeing in a strong alkali state by a special method) of the particle size of 0.01 to 0.25 ㎛. 삭제delete 제1항에서 있어서, 밀폐형 제트 염색기를 사용하는 것을 특징으로 하는 배트염료를 이용한 고기능성 합성섬유의 염색방법.The method of dyeing high-performance synthetic fibers using bat dyes according to claim 1, characterized in that a closed jet dyeing machine is used. 제1항에서 있어서, 염색 액비를 1:5 내지 20으로 설정하는 것을 특징으로 하는 배트염료를 이용한 고기능성 합성섬유의 염색방법.The method for dyeing a highly functional synthetic fiber using a bat dye according to claim 1, wherein the dyeing liquid ratio is set at 1: 5 to 20. 제1항에서 있어서, 환원제로서 Na2S2O4와 Na2CO3를 각각 5 내지 20 g/l로 사용하는 것을 특징으로 하는 배트염료를 이용한 고기능성 합성섬유의 염색방법.According to claim 1, Na 2 S 2 O 4 and Na 2 CO 3 as a reducing agent, characterized in that the dyeing method of high-performance synthetic fibers using a bat dye, characterized in that each 5 to 20 g / l. 제1항에서 있어서, 환원제 투입온도를 80 내지 100℃로 하는 것을 특징으로 하는 배트염료를 이용한 고기능성 합성섬유의 염색방법.The method of dyeing a highly functional synthetic fiber using a bat dye, characterized in that the reducing agent input temperature is 80 to 100 ℃. 제5항에서 있어서, Na2S2O4를 먼저 투입한 후 Na2CO3를 투입하는 것을 특징으로 하는 배트염료를 이용한 고기능성 합성섬유의 염색방법.The method of dyeing a highly functional synthetic fiber using a bat dye according to claim 5, wherein Na 2 S 2 O 4 is added first, followed by Na 2 CO 3 . 제1항에서 있어서, 분산제와 균염제를 각각 0.1 내지 1 g/l로 사용하는 것을 특징으로 하는 배트염료를 이용한 고기능성 합성섬유의 염색방법.The method of dyeing high-performance synthetic fibers using bat dyes according to claim 1, wherein dispersing and leveling agents are used at 0.1 to 1 g / l, respectively. 제1항에서 있어서, 염색 온도를 125 내지 130℃로 하는 것을 특징으로 하는 배트염료를 이용한 고기능성 합성섬유의 염색방법.The method of dyeing high-performance synthetic fibers using a bat dye, characterized in that the dyeing temperature is 125 to 130 ℃. 제1항에서 있어서, 산화제로서 H2O2를 0.1 내지 1 g/l로 사용하는 것을 특징으로 하는 배트염료를 이용한 고기능성 합성섬유의 염색방법.The method of dyeing a highly functional synthetic fiber using a bat dye, according to claim 1, wherein H 2 O 2 is used at 0.1 to 1 g / l as an oxidizing agent. 제1항에서 있어서, 산화공정을 125 내지 130℃에서 수행하는 것을 특징으로 하는 배트염료를 이용한 고기능성 합성섬유의 염색방법.The method of dyeing a highly functional synthetic fiber using a bat dye, characterized in that the oxidation process is carried out at 125 to 130 ℃.
KR1020060083249A 2006-08-31 2006-08-31 Process for dyeing high functional synthetic fiber using vat dye KR100669082B1 (en)