KR0145117B1 - Epoxy resin mortar - Google Patents

Epoxy resin mortar

Info

Publication number
KR0145117B1
KR0145117B1 KR1019960001581A KR19960001581A KR0145117B1 KR 0145117 B1 KR0145117 B1 KR 0145117B1 KR 1019960001581 A KR1019960001581 A KR 1019960001581A KR 19960001581 A KR19960001581 A KR 19960001581A KR 0145117 B1 KR0145117 B1 KR 0145117B1
Authority
KR
South Korea
Prior art keywords
weight
epoxy resin
resin mortar
composition
resin
Prior art date
Application number
KR1019960001581A
Other languages
Korean (ko)
Other versions
KR970059141A (en
Inventor
김상양
Original Assignee
현기일
배성물산주식회사
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 현기일, 배성물산주식회사 filed Critical 현기일
Priority to KR1019960001581A priority Critical patent/KR0145117B1/en
Publication of KR970059141A publication Critical patent/KR970059141A/en
Application granted granted Critical
Publication of KR0145117B1 publication Critical patent/KR0145117B1/en

Abstract

본 발명은 에폭시 수지 모르타르 시공방법에 관한 것으로서, 더욱 상세하게는 에폭시 수지 모르타르 조성물과 자연석 또는 인조석 규사를 배합하여 이를 포설한 다음 압착미장하고 경화시킨 표면층에 에폭시 수지를 기본수지로 한 응집성 성형코팅재를 도포함으로써 표면 공극만을 일정한 두께로 메꾸어 평면 또는 엠보싱 상태를 갖게하여 미관을 향상시킬 수 있는 에폭시 수지 모르타르 시공방법에 관한 것이다.The present invention relates to a method for constructing an epoxy resin mortar, and more particularly, an epoxy resin mortar composition and natural stone or artificial silica sand are blended and laid thereon, and then pressed and cured to form a cohesive molding material having an epoxy resin as a base resin. The present invention relates to an epoxy resin mortar construction method capable of filling a surface void only to a certain thickness to apply a flat or embossed state to improve aesthetics.

Description

에폭시 수지 모르타르 시공방법Epoxy Resin Mortar Construction Method

본 발명은 에폭시 수지 모르타르 시공방법에 관한 것으로서, 더욱 상세하게는 에폭시 수지 모르타르 조성물과 자연석 또는 인조석 규사를 배합하여 이를 포설한 다음 압착미장하고 경화시킨 표면층에 에폭시 수지를 기본수지로 응집성 성형코팅재를 도포함으로써 표면 공극만을 일정한 두께로 메꾸어 평면 또는 엠보싱 상태를 갖게하여 미관을 향상시킬 수 있는 에폭시 수지 모르타르 시공방법에 관한 것이다.The present invention relates to a method for constructing an epoxy resin mortar, and more particularly, an epoxy resin mortar composition and natural stone or artificial silica sand are mixed and laid thereon, and then coated with a cohesive molding coating material with epoxy resin as a base resin on the surface layer which is pressed and cured. The present invention relates to an epoxy resin mortar construction method capable of filling a surface void only to a certain thickness to have a flat or embossed state to improve aesthetics.

일반적으로 사용되고 있는 수지 모르타르는 에폭시 수지를 기본으로 한 것이 대부분이며, 이와같이 조성으로 이루어진 에폭시 수지 모르타르를 시공할 때에는 이를 포설 미장한 후 공극 전체를 메꾸어 주는 방법을 사용하였다. 이와같은 방법으로 수지 모르타르를 시공하는 경우 마무리 상태가 정교하지 못하고 투박할 뿐만 아니라 에폭시 수지가 고가인데도 불구하고 다량 사용해야 하므로 고강도 및 내충격성을 요하는 경우에 미관에는 상관없이 시공되어져 온 실정이다.Resin mortars generally used are based on epoxy resins, and when constructing epoxy resin mortars composed of such compositions, they are laid and then filled with voids. When the resin mortar is constructed in this manner, the finishing state is not precise and not only coarse, but even though the epoxy resin is expensive, it must be used in large quantities, so it has been constructed regardless of aesthetics when high strength and impact resistance are required.

미적으로 투박한 상태를 가질 수 밖에 없었던 이유는 일정한 두께로 미장시공한 다음 높은 강도를 유지시켜 주기 위해서도 공극을 메꾸어주지만 에폭시 수지 자체가 셀프레벨링 타입(self levelling type)으로 생산시공이 용이하여 모르타르층 전체를 규사가 침지된 상태로 마루리할 수 밖에 없었기 때문이다.The reason why it had to be aesthetically coarse was to fill the pores in order to maintain high strength after plastering with a certain thickness, but the epoxy resin itself is a self-leveling type, which is easy to produce and manufacture. This is because it had no choice but to marry the silica.

또한 셀프레벨링 타입은 수평선상의 수지 표면과 수지 모르타르 시공면이 고르게 일치되게 할 수 없기 때문에 정교함과 미적인 감각을 살릴 수 없었다.In addition, the self-leveling type could not make the resin surface on the horizon and the surface of the resin mortar evenly match, so it could not make use of the sophistication and aesthetic sense.

한편, 최근에 이르러서도 건물 내외부 바닥이나 벽면 등에는 각종 타일류가 이용되고 있고, 석재 대리석이 그 주종을 이루고 있다. 이 제품들은 내후성, 내구성 및 내마모성이 뛰어난 제품들로서 오래도록 전통성을 유재하고 있으나, 고도의 산업화로 생활환경이 변화함으로써 새로운 감각의 미적 성향을 추구하는 현대인들에게 종래의 수지 모르타르의 시공방법으로는 상기와 같은 욕구를 충족시킬 수 없다.On the other hand, in recent years, various tiles are used for interior and exterior floors and wall surfaces, and stone marble is mainly used. These products are excellent in weatherability, durability and abrasion resistance, and they have long-established traditions.However, the conventional resin mortar application method is the method of construction of resin mortar for the modern people who pursue a new sense of aesthetics by changing the living environment with high industrialization. You cannot meet the same needs.

따라서, 본 발명자는 상기와 같은 종래의 수지 모르타르 시공방법의 문제점을 해결하기 위하여 노력한 결과 통상의 에폭시 수지 모르타르 조성물과 자연석 또는 인조석 규사를 배합하여 포설한 뒤 압착 미장하여 경화시킨 표면층을 응집성 성형코팅재로 메꾸어 줌으로써 본 발명을 완성하였다.Accordingly, the present inventors endeavored to solve the problems of the conventional resin mortar construction method as described above, and the conventional epoxy resin mortar composition and natural stone or artificial silica sand are mixed and laid, and then pressed and cured to form a cohesive molding coating material. The present invention has been completed by filling up.

본 발명은 에폭시 수지 모르타르 시공 후 그 표면층을 응집성 성형코팅재로 메꾸어 줌으로써 미관을 향상시키고 내구성 및 내충격성이 우수하도록 한 에폭시 수지 모르타르의 시공방법을 제공하는데 목적이 있다.An object of the present invention is to provide a method for constructing an epoxy resin mortar, which improves aesthetics and has excellent durability and impact resistance by filling the surface layer with a cohesive molding coating material after construction of the epoxy resin mortar.

이하, 본 발명을 상세히 설명하면 다음과 같다.Hereinafter, the present invention will be described in detail.

본 발명은 에폭시 수지를 기본수지로 하고 여기에 경화제, 경화촉진제 및 안료등의 첨가제를 혼합하여 이루어진 에폭시 수지 모르타르를 시공하는 방법에 있어서, 상기의 에폭시 수지 모르타르 조성물에 자연석 또는 인조석 규사를 배합하고 포설한 다음 압착미장하고 경화시킨 후, 그 표면층에 응집성 성형코팅재를 일정 두께로 메꾸는 것을 그 특징으로 한다.The present invention is a method for constructing an epoxy resin mortar formed by mixing an epoxy resin as a base resin and adding additives such as a curing agent, a curing accelerator, and a pigment to the epoxy resin mortar composition, wherein natural stone or artificial silica sand is blended and laid. After pressing and curing and curing, the surface layer is characterized by filling a cohesive molding coating material in a predetermined thickness.

그리고, 상기 응집성 성형코팅재로는 에폭시 수지 70∼80 중량%, 가소제 3∼5 중량%, 치소제 4∼5 중량%, 비반응성 희석재 14∼16 중량% 및 소포제 0.05∼0.1 중량%로 이루어진 주재 100 중량부와 이에 대하여 경화제 50∼60%, 레진 아닥트제 7∼15 중량% 및 촉진제 25∼33 중량%로 이루어진 경화제 50 중량부로 이루어진 조성물을 사용하는 것에도 그 특징이 있다.The cohesive molding coating material is composed of 70 to 80% by weight of epoxy resin, 3 to 5% by weight of plasticizer, 4 to 5% by weight of plasticizer, 14 to 16% by weight of non-reactive diluent and 0.05 to 0.1% by weight of antifoaming agent. It is also characterized by the use of a composition comprising 100 parts by weight and 50 parts by weight of a curing agent composed of 50 to 60% of a curing agent, 7 to 15% by weight of a resin adduct and 25 to 33% by weight of an accelerator.

이와같은 본 발명을 더욱 상세하게 설명하면 다음과 같다.The present invention will be described in more detail as follows.

본 발명은 에폭시 수지 모르타르 시공 후 응집성 성형코팅재를 사용함으로써 미관을 향상시키고 용도에 따라 어느 곳에든 다양하게 활용이 가능한 에폭시 수지 모르타르의 시공방법에 관한 것을로서, 본 발명에서 사용되는 수지 모르타르는 통상의 조성으로 이를 구체적으로 살펴보면 ;The present invention relates to a method for constructing an epoxy resin mortar that can improve aesthetics by using a cohesive molding coating material after construction of epoxy resin mortar and can be variously used depending on the use. The resin mortar used in the present invention is conventional Looking specifically at the composition;

에폭시 수지 85∼90 중량%, 반응성 희석제 5∼10 중량%, 가소제 2∼4 중량%, 레벨링제 0.05∼0.1 중량%, 소포제 0.05∼0.1 중량 % 및 자외선방지제 0.8∼1.3 중량%로 이루어진 제1 조성물 100 중량부와 이에 대하여 경화제 55∼65 중량%, 레진 아닥트제 7∼15 중량% 및 촉진제 27∼40 중량%로 이루어진 제2 조성물 50 중량부 및 무기안료 또는 유기안료 1∼3 중량부로 이루어진다.First composition consisting of 85 to 90 wt% epoxy resin, 5 to 10 wt% reactive diluent, 2 to 4 wt% plasticizer, 0.05 to 0.1 wt% leveling agent, 0.05 to 0.1 wt% antifoaming agent and 0.8 to 1.3 wt% sunscreen 100 parts by weight with respect to 50 parts by weight of the second composition consisting of 55 to 65% by weight of the curing agent, 7 to 15% by weight of the resin adduct and 27 to 40% by weight of the accelerator, and 1 to 3 parts by weight of the inorganic pigment or the organic pigment.

그 다음, 상기 에폭시 수지 조성물 100 중량부와 자연석 또는 인조석 500∼1000 중량부를 혼합교반시킨다.Next, 100 parts by weight of the epoxy resin composition and 500 to 1000 parts by weight of natural or artificial stone are mixed and stirred.

그리고 나서, 이를 콘크리트면에 2∼15mm 두께로 포설하고 압착미장한다.Then, it is laid on the concrete surface with a thickness of 2 to 15 mm and pressed and plastered.

한편, 이를 벽면에 시공할 경우에는 2∼3mm 두께로 포설하고 압착미장한다.On the other hand, when it is installed on the wall surface is installed in 2-3mm thickness and crimped plastering.

여기서, 에폭시 수지 모르타르 조성이나 응집형 성형코팅재에서 사용하는 에폭시 수지 중간체의 구조식은 다음과 같다.Here, the structural formulas of the epoxy resin intermediates used in the epoxy resin mortar composition and the aggregation type coating material are as follows.

상기 식에서 n=0 이다.Where n = 0.

본 발명에서 사용되는 에폭시 수지 중간체의 구조식에서 n=0인 것은 에폭시 수지 모르타르 제조시 사용되는 에폭시 수지는 액상이어야 하는 바, 만일 n=0이 아닌 경우 고형의 수지상이 되기 때문이다.In the structural formula of the epoxy resin intermediate used in the present invention, n = 0 is because the epoxy resin used in the production of the epoxy resin mortar should be a liquid phase, if it is not n = 0, it becomes a solid resin phase.

상기와 같은 에폭시 기본수지 외에 이소프로필렌티페놀 글리시딜에테르를 소량 혼합하여 사용할 수도 있다.In addition to the above epoxy base resins, a small amount of isopropylene thiphenol glycidyl ether may be mixed and used.

그리고, 반응성 희석제로는 에폭시기를 갖고 있는 단분자형으로서, 폴리프로필렌글리콜 디글리시딜을 단독으로 사용하거나 안정성이 높은 부틸글리시딜에테르와 1:1로 혼합 사용할 수 있다.As the reactive diluent, a monomolecular type having an epoxy group, polypropylene glycol diglycidyl may be used alone or in a 1: 1 mixture with high butylglycidyl ether.

가소제는 물성의 사소성 내지는 안정성을 높이기 위해 사용하고, 레벨링제로는 폴리실록세니계에 에스테르계의 고비점 용제가 혼합된 것으로서 표면레벨링 상태를 양호하게 하여 수지 표면에 아민이 상용성을 갖지 않고 상대습도 변화에 따라 위로 뜨는 현상, 즉 아민브러쉬 현상이 나타나지 않도록 함으로써 재코팅시 접착을 도모할 수 있도록 한다.The plasticizer is used to increase the plasticity or stability of the physical properties. The leveling agent is a polysiloxane-based high boiling point solvent mixed with an ester. The surface leveling is good, and the amine is not compatible with the surface of the resin. It is possible to promote adhesion during recoating by preventing the phenomenon of floating up according to the change, that is, the amine brush phenomenon.

소포제로는 폴리실록세니 계열로서 조성물 내지 기포의 형성을 방지하고, 자외선방지제로는 예컨데 폴리-〔(6-몰폴리노-S-트리아진-2, 4-디일)-(2, 2, 6, 1-테트라에틸-4-피페리닐) 이미노-헥사메틸렌-(2, 2, 6, 6-테트라메틸)-이미노〕를 사용한다.The antifoaming agent is a polysiloxane-based series to prevent the formation of the composition or bubbles, and as the sunscreen, for example, poly-[(6-morpholino-S-triazine-2, 4-diyl)-(2, 2, 6, 1-tetraethyl-4-piperidyl) imino-hexamethylene- (2, 2, 6, 6-tetramethyl) -imino] is used.

이와같은 조성으로 이루어진 에폭시 수지 모르타르 조성물중의 제1조성물의 각 성분의 함량이 상기 범위 미만이면 결성자체가 이루어지지 않으며, 상기 함량을 초과하여 사용하면 조성물내에서 상용성이 낮을 뿐만 아니라 경도, 인장강도, 굴곡강도 및 압축응력이 저하되는 등 물성이 나빠지게 된다.If the content of each component of the first composition in the epoxy resin mortar composition having such a composition is less than the above range, the formation itself is not formed, and when used in excess of the above content, not only the compatibility in the composition is low, but also the hardness and tension Physical properties are deteriorated, such as a decrease in strength, flexural strength and compressive stress.

또한, 상기 에폭시 수지 모르타르의 제1조성물 중 안료를 첨가할 수 있는데, 이러한 안료는 무기 또는 유기안료로서 1∼3 중량부 사용한다. 만일 안료의 상용량이 1중량부 미만이면 반투명해지고, 3중량부를 초과하면 불투명해진다.In addition, a pigment may be added in the first composition of the epoxy resin mortar, which is used in an amount of 1 to 3 parts by weight as an inorganic or organic pigment. If the compatible amount of the pigment is less than 1 part by weight, it becomes translucent and if it exceeds 3 parts by weight, it becomes opaque.

이때 무기안료로는 0.2∼0.4mμ크기의 것, 더욱 크게는 25mμ정도로 큰 것을 사용할 수도 있으며, 구체적인 예로는 크로뮴(Chromium) (그린), 카드뮴(Cadmium) (레드), 이산화티탄 또는 크로메이트(Chromates), 페로시아나이드(Ferrocyanides) (청), 설파이드(Sulfide), 옥사이드(Oxides), 실리케이트(Silicates), 카본블랙이 있다.The inorganic pigments may be 0.2 ~ 0.4mμ in size, and larger ones such as 25mμ in size. Specific examples include chromium (green), cadmium (red), titanium dioxide or chromates. , Ferrocyanides (blue), Sulphide, Oxides, Silicates, Carbon Black.

이같은 안료는 여러 금속과 함께 상호침전법(Coprecipitation)을 적용하여 색상을 변경할 수 있다.Such pigments can be changed in color by applying coprecipitation with several metals.

그리고, 유기안료로는 프탈로시아닌계를 비롯한 통상적인 여러 종류의 것을 사용할 수 있으며, 특히 퀸아크리딘(Quinacridine)계 안료를 단독 또는 상기의 무기안료와 함께 혼합 사용할 수도 있다.As the organic pigment, various kinds of conventional pigments, including phthalocyanine, may be used, and in particular, a quinacridine pigment may be used alone or in combination with the inorganic pigment.

한편, 에폭시 수지 모르타르 조성물 제2조성물인 경화제 조성에 있어서, 사용되는 경화제는 아민계 경화제인 폴리옥시 프로필렌 아민이며, 레진 아닥트제는 상기의 에폭시 기본수지를 사용하며, 경화촉진제로는 몰수가 없는 노닐페놀을 사용한다. 이때, 경화촉진제로서 몰수가 없는 노닐페놀을 사용한 것은 경화시 발열로 인한 황변 또는 자외선에 의해 발생되는 노화현상을 줄이기 위해서이다.On the other hand, in the composition of the curing agent which is the second composition of the epoxy resin mortar composition, the curing agent used is polyoxypropylene amine which is an amine curing agent, and the resin adduct agent uses the epoxy base resin described above, and the curing accelerator has no molarity. Use nonylphenol. In this case, nonylphenol, which is not molar, is used as a curing accelerator to reduce the aging phenomenon caused by yellowing or ultraviolet rays due to heat generation during curing.

또한, 경화촉진제로는 피페페라진계 혼합물 변성 아민을 온도 편차에 따라 5∼10 중량% 조절하여 사용하는 바, 10℃ 이하에서는 10 중량% 미만으로, 20∼30℃에서는 5 중량% 이내로 사용하는 것이 바람직하다.In addition, as a curing accelerator, it is used to adjust the piperazine-based mixture modified amine by 5 to 10% by weight according to the temperature variation, less than 10% by weight at 10 ℃ or less, 5% by weight at 20 to 30 ℃. desirable.

한편, 상기와 같이 수지 모르타르를 시공한 후 공극을 메꾸어주기 위해서 본 발명에서는 수지 모르타르 시공후에 표면에 응집성 성형 코팅재를 코팅한다.On the other hand, in order to fill the pores after the construction of the resin mortar as described above, in the present invention, the cohesive molding coating material is coated on the surface after the construction of the resin mortar.

종래에는 일반적인 도료제품에 흐름성을 방지하기 위하여 치소성(thiso)을 갖고 있는 실리콘 디옥사이드계를 원료로 이용하여 왔는데, 이액형 수지, 특히 에폭시계 성형제품 원료로 사용하기에는 까다로운 특성을 갖고 있다.Conventionally, in order to prevent flowability in general paint products, silicon dioxide based on the tooth (thiso) has been used as a raw material, it has a characteristic that is difficult to use as a two-component resin, especially epoxy-based molded product raw materials.

그리고, 고점도의 응집성을 갖기 위해서는 많은 양을 첨가해야 되고, 이에 따라 에폭시 본래의 원하는 물성을 갖기 어렵다.And, in order to have high viscosity cohesiveness, a large amount must be added, and thus, it is difficult to have the desired physical properties of epoxy.

따라서, 본 발명의 응집성 성형제는 주재 성분에 소량의 치소제를 첨가하여 흐름상태외로의 물성을 갖게하고 경화제를 에폭시 기본수지와 70℃에서 아닥트시키는데, 이때 대기 중에 있는 수분을 자연스럽게 흡수한다.Therefore, the coagulant molding agent of the present invention adds a small amount of a plasticizer to the main component to give physical properties out of the flow state, and adsorbs the curing agent at 70 ° C. with the epoxy base resin, and naturally absorbs moisture in the air.

여기서, 응집성 성형코팅재의 조성은 주재와 경화제 성분으로 나뉘며, 주재는 상기 구조식으로 표시되는 에폭시 수지 70∼80 중량%, 가소제 3∼5 중량%, 치소제 4∼5 중량%, 비반응성 희석제 14∼16 중량% 및 소포제 0.05∼0.1 중량%로 이루어진다.Here, the composition of the cohesive molding coating material is divided into a main material and a hardener component, the main material is 70 to 80% by weight epoxy resin, 3 to 5% by weight plasticizer, 4 to 5% by weight plasticizer, non-reactive diluent 14 ~ 16 weight% and antifoaming agent 0.05 to 0.1 weight%.

그리고, 경화제 성분은 경화제 50∼60 중량%, 레진 아닥트제 7∼15 중량%, 촉진제 25∼33중량%로 이루어진다.And a hardening | curing agent component consists of 50 to 60 weight% of hardening | curing agents, 7 to 15 weight% of resin adads, and 25 to 33 weight% of accelerators.

상기와 같은 주재 100 중량부와 경화제 50 중량부를 혼합하고, 현장시공시 디에틸렌트리아민 또는 트리에틸렌 테트라아민을 0.5∼1.0 중량% 첨가 혼합하여 응집성을 갖게 한 다음 모르타르 표면층에 성혀코팅한다.100 parts by weight of the main material as described above and 50 parts by weight of a curing agent are mixed, and 0.5 to 1.0% by weight of diethylenetriamine or triethylene tetraamine is added and mixed to make cohesive and then coated on a mortar surface layer.

여기서, 주재 조성물중 기본이 되는 에폭시 수지는 상기 구조식(1)로 표시되며, 여기에 염소분이 함유된 에폭시 기본 수지를 일부 혼합 사용한다. 이때 염소분이 함유된 에폭시 기본수지는 응집성을 갖게하는 부분적인 역할을 한다.Here, the epoxy resin as a base in the main composition is represented by Structural Formula (1), and a part of the epoxy base resin containing chlorine is mixed therein. At this time, epoxy base resin containing chlorine plays a part in making cohesive.

그리고, 가소제로는 디부틸프탈레이트를 사용하는데, 이는 가소성을 갖게 하지만 비휘발성 타입으로서 디에틸렌트리아민이나 트리에틸렌테트라아민 첨가시 응집성을 도모한다.As the plasticizer, dibutyl phthalate is used, which gives plasticity but promotes cohesiveness when diethylenetriamine or triethylenetetraamine is added as a nonvolatile type.

또한, 치소제로는 실리콘옥사이드 단독 또는 칼리드리아 아스베스토를 1:1로 혼합 사용하여 수지에 치소성을 갖게 하는데, 구체적으로는 실리콘디옥사이드나 칼리드리아 아스베스토로서 비중이 아주 낮아 생산시 삼본 롤러를 이용하여 밀링(milling)하는데 있어서 압착정도를 파악하여 치소성이 감소되지 않도록 유의해야 하며, 진공탈포기를 이용하여 기포를 제거해야 한다.In addition, as the dentifrice, silicon oxide alone or Calibria asbestos is mixed in a 1: 1 ratio to give plasticity to the resin. When milling (milling) to determine the degree of compression to be careful not to reduce the plasticity, and vacuum degassing should be used to remove the bubble.

비반응성 희석제로는 크실렌을 사용하는데, 지점도 성형타입에서 휘발성과 용해력이 낮아 물성에 안정성이 높고 치소제와의 흡습력 및 상용성이 좋아 치소성을 더욱 증대시킨다.Xylene is used as a non-reactive diluent, which has high volatility and dissolvability in the branched molding type, so it has high stability in physical properties, good hygroscopicity and compatibility with the plasticizer, and further increases plasticity.

그리고, 소포제로는 폴리실록세니계 혼합물을 사용하는 바, 이는 발포성이 강한 소포제로서 수지내에 기포형성을 방지한다.As the antifoaming agent, a polysiloxane mixture is used, which is a highly foamable antifoaming agent, which prevents foaming in the resin.

한편, 응집성 성형코팅재 조성중 경화제 성분 조성은 경화제로서 아민계 경화제인 폴리옥시프로필렌아민을 사용하고, 레진 아닥트제는 에폭시 기본수지이며, 경화촉진제로는 피레라진계 혼합물 3급 아민과 노닐페놀을 사용하는데 이때 노닐페놀 촉진제는 몰수가 없는 타입으로서 반응발열시 황변이나 노화현상을 줄이기 위해서 사용한다.In the composition of the cohesive molding coating material, the composition of the curing agent is polyoxypropyleneamine, which is an amine curing agent, as the curing agent, the resin adduct is an epoxy base resin, and the curing accelerator is a tertiary amine mixture and a nonylphenol. The nonylphenol accelerator is a type that can not be moles and is used to reduce yellowing or aging during the heating of the reaction.

또한, 본 발명에서 경화제 아닥트 방법으로 아닥트 예배온도는 60℃에서 반응이 시작되는 것이 적합하고 상승온도가 저하하면서 수분을 흡습하므로서, 사용시 트리에틸렌테트라아민이나 디에틸렌트리아민을 첨가하여 수분과 반응하면서 강한 응집력을 갖도록 한다.In addition, in the present invention, the adduct worshiping temperature in the method of advent hardening in the present invention is suitable for starting the reaction at 60 ° C. and absorbing moisture while lowering the rising temperature, so that triethylenetetraamine or diethylenetriamine may be added during use. React and have a strong cohesion.

상기와 같은 응집성 성형코팅재 조성 중 각 성분의 함량이 상기 함량 미만이면 구성물의 결성이 이루어지지 않고, 그 함량을 초과하면 물성의 특성이 약화된다.If the content of each component in the composition of the cohesive molding coating as described above is less than the content is not formed of the composition, if the content exceeds the properties of the physical properties are weakened.

한편, 에폭시 수지 모르타르의 시공에 있어서, 상술한 바와 같은 에폭시 수지 모르타르 조성에 통상의 방법대로 자연석 규사 또는 인조석 석재조각을 입자크기 0.1∼5mm로 10∼20 중량부 혼합한 뒤 에폭시 프라이머를 도포한 콘크리트 면위에 두께 0.3∼15mm로 포설한 다음, 일정한 압력을 가하여 기계적 연식미장 또는 손으로 미장한다.On the other hand, in the construction of epoxy resin mortar, 10 to 20 parts by weight of natural stone silica sand or artificial stone pieces with a particle size of 0.1 to 5 mm by mixing the epoxy resin mortar composition as described above in the usual manner, and then coated with epoxy primer Lay 0.3 to 15mm thick on the surface, and then apply it by mechanical pressure plastering or by hand.

그리고 나서, 에폭시 수지 모르타르가 경화된 표면층에 응집성 성형코팅재의 주재와 경화제를 중량비 100 : 50 으로 하여 혼합한 뒤 트리에틸렌테트라아민을 0.5∼1.0 중량% 첨가하고 교반하여 강한 응집성을 갖도록 한다. 이를 모르타르 표면층에 부어 고무헤라를 이용하여 골고루 얇게 펴준 다음, 부직포 롤러를 이용하여 롤링함으로써 표면층이 정교하게 엠보싱 상태를 갖도록 하는데 부직포 롤러 모양에 따라 표면은 여러 모양으로 나타낼 수 있다.Then, the main material of the cohesive molding coating material and the curing agent are mixed in a weight ratio of 100: 50 to the surface layer on which the epoxy resin mortar is cured, and then 0.5 to 1.0% by weight of triethylenetetraamine is added and stirred to have strong cohesiveness. This is poured into a mortar surface layer and evenly spread using a rubber hera, and then rolled using a nonwoven roller to have a finely embossed surface layer. The surface may be represented in various shapes depending on the shape of the nonwoven roller.

이와 같이 마무리된 상태에서 용도에 맞게 각각의 내산성, 내후성, 내마모성, 내충격성 등의 특성을 부여 상도코팅을 얇게 처리할 수 있는데, 상도코팅은 에폭시계, 우레탄계 또는 우레탄에 아크릴을 블렌딩시킨 타입일 때만 접착이 원만하다.In this finished state, each acid-resistance, weather resistance, abrasion resistance, impact resistance, etc. can be given to the application, and the top coat can be treated thinly.The top coat is only epoxy type, urethane, or urethane-based acrylic blended type only. Adhesion is smooth.

상기한 바와 같이 에폭시 수지 모르타르를 시공하는 경우 제반물성이 우수하면서도 외관이 미려하고 내약품서도 우수하여 종래의 모르타르 시공방법보다 매우 유용하게 이용할 수 있다.As described above, when the epoxy resin mortar is constructed, the physical properties are excellent, the appearance is beautiful and the chemical resistance is excellent, and thus it can be used more effectively than the conventional mortar construction method.

이하, 본 발명을 실시예에 의거 상세히 설명하면 다음과 같은 바, 본 발명이 실시예에 의해 한정되는 것은 아니다.Hereinafter, the present invention will be described in detail with reference to Examples, but the present invention is not limited by the Examples.

[제조예1][Production Example 1]

에폭시 수지 모르타르 조성물Epoxy Resin Mortar Composition

상기 조성에서,In the composition,

(1) 에폭시 기본 수지 : 에필클로로하이드린과 비스페놀 A의 축합생성물로 끈적끈적한 액상으로서, 에폭시 당량 190∼195이고, 접도(25℃) 2,500∼3,000 센티포이즈, 색상(투명)수지(gardner)는 0.5 Max, 비중(20℃)은 1.17, 굴절율(20℃)는 1.5713인 국도화학 제품.(1) Epoxy base resin: Condensation product of epichlorohydrin and bisphenol A, a sticky liquid, epoxy equivalent of 190 to 195, abutment (25 ° C) 2,500 to 3,000 centipoise, color (transparent) resin (gardner) Kukdo Chemical's 0.5 Max, specific gravity (20 ℃) is 1.17, refractive index (20 ℃) is 1.5713.

(2) 반응성 희석제 : 폴리프로필렌글리콜 디글리시딜, 일본 동도화성 제품(2) Reactive diluent: polypropylene glycol diglycidyl, Japan Dowha Chemical

(3) 가소제 : 디부틸프탈레이트, 애경유지 제품(3) Plasticizers: dibutyl phthalate, Aekyung oil and fat products

(4) 소포제 : 폴리실록세니계 혼합물, 독일 BYK사 제품(4) Defoamer: Polysiloxane compound, Germany BYK

(5) 레벨링제 : 포리실록세니계 혼합물, 독일 BYK사 제품(5) Leveling agent: Polysiloxane-based mixture, manufactured by BYK of Germany

(6) 자외선 방지제 : UV-3346, 미국 시아나미드사 제품(6) UV inhibitor: UV-3346, manufactured by Cyanamide, USA

(7) 경화제 : 폴리옥시프로필렌 아민, 미국 텍샤코사 제품(7) Curing agent: Polyoxypropylene amine, manufactured by Texark, USA

(8) 레진 아닥트제 : 기본 에폭시 수지, YD-128, 국도화학 제품(8) Resin adduct: Basic epoxy resin, YD-128, Kukdo Chemical

(9) 노닐 페놀, 이탈리아 와카사 제품(9) Nonyl Phenolic, Product from Wakasa, Italy

(10) 피페라진 혼합물, 미국 텍샤코사 제품(10) Piperazine Mixture, manufactured by Texark, USA

상기 제1조성물〔점도(20℃) 3,000 cps, 비중 1.22〕과 제2조성물〔점도(20℃) 350cps, 비중 1.13〕을 중량비 100 : 50으로 혼합하고, 여기에 안료를 1∼3 중량부 혼합하여 에폭시 수지 모르타르 조성물을 얻었다.The first composition [viscosity (20 ° C.) 3,000 cps, specific gravity 1.22] and the second composition [viscosity (20 ° C.) 350 cps, specific gravity 1.13] are mixed in a weight ratio of 100: 50, and the pigment is mixed in an amount of 1 to 3 parts by weight. To obtain an epoxy resin mortar composition.

상기 조성에서In the composition

(11) 기본수지 : 에피클로로하이드린과 비스페놀 A의 축합생성물로서 끈적끈적한 액상. 에폭시 당량 184∼190, 점도(25℃), 2,000∼2,500 cps, 색상 반투명수지(gardner)는 0.5Max, 비중(20℃) 1.15, 굴절율(20℃)이 1,5710안 국도화학 제품.(11) Basic resin: A sticky liquid as a condensation product of epichlorohydrin and bisphenol A. Epoxy equivalent of 184 to 190, viscosity (25 ℃), 2,000 to 2,500 cps, color semitransparent resin (gardner) 0.5Max, specific gravity (20 ℃) 1.15, refractive index (20 ℃) of 1,5710 Kukdo Chemical.

(12) 중점도 타입으로 염소분을 함유하고 있음. YD-115CA, 국도화학 제품(12) Medium viscosity type containing chlorine. YD-115CA, Kukdo Chemical

(13) 실리콘 디옥사이드 또는 RG-244(13) silicon dioxide or RG-244

(14) 크실렌(14) xylene

상기 주재 〔점도(20℃) 2,500 cps, 비중 1.2〕와 경화제〔점도(20℃) 350 cps, 비중 1.13〕를 중량비 100 : 50으로 혼합하고, 여기에 트리에틸렌테트라아민 0.5∼1g을 첨가하여 응집성 성형코팅재를 얻었다.The main material [viscosity (20 degreeC) 2,500 cps, specific gravity 1.2] and the hardening | curing agent [viscosity (20 degreeC) 350 cps, specific gravity 1.13] are mixed by weight ratio 100: 50, and 0.5-1 g of triethylene tetraamine is added here, and it is cohesive A molding coating material was obtained.

[실시예]EXAMPLE

먼저 콘크리트 양생은 상온에서 15일 이상지나 함수율이 8% 이하인가 또는 콘크리트 표면강도는 180 이상인가 확인한 후 표면에 오염부위, 요철, 레이탄스를 제거하여 표면 처리 작업이 끝나면 에폭시 프라이머를 표면 밀도에 따라 1㎡ 기준 0.2∼0.3㎏ 정도를 롤러를 이용 골고루 침투하도록 발라준다.First, after curing the concrete for 15 days or more at room temperature but with a water content of 8% or less, or concrete surface strength of 180 or more, remove contaminants, irregularities and latans on the surface. Apply 0.2 to 0.3 ㎏ based on 1㎡ to penetrate evenly using rollers.

프라이머가 경화되었는가 확인 한 후 상기 제조에 1에 따라 제조된 수지 모르타르층을 시공하는데 프라이머가 도포되어 있는 위에 0.2∼0.3mm 두께로 얇게 하여 준 다음, 자연석(규사) 또는 인조석(칼라규사) 중 원하는 석재조각 : 제조예 1의 수지 모르타르 조성물의 비율이 100 : 10∼20 중량 % 되도록 혼합 교반하여 규정된 두께로 포설압착 미장하였다.After confirming that the primer was cured, the resin mortar layer prepared according to the above 1 was prepared to be thinned to a thickness of 0.2 to 0.3 mm on which the primer was applied, and then selected from natural stone (silica sand) or artificial stone (color silica sand). Stone carving: Mixing and stirring so that the ratio of the resin mortar composition of Preparation Example 1 was 100: 10 to 20% by weight, the pressure was laid in a prescribed thickness.

경화시간은 재작업이 가능한 지촉건조시간은 20℃에서 8∼12 시간이지만, 경화건조 상태를 확인해야 하며 점검이 끝나면 상기 제조예 2에 따라 제조된 응집성 성형코팅재를 상기 기술한 바와 같이 응집상태를 체크한 후 표면층에 발라 고무헤라를 이용 얇게 펴준 다음 부직포 롤러를 이용 로울링하여 마무리하였다.Although the curing time is re-workable, the dry touch time is 8 to 12 hours at 20 ° C., but the curing dry state should be checked and the cohesive molding coating material prepared according to Preparation Example 2 after the inspection is finished, as described above. After checking, the surface layer was thinly spread using a rubber hera, and then finished by rolling with a nonwoven roller.

[실험예]Experimental Example

상기 실시예에 따라 수지 모르타르를 시공한 후, 시공면 중 코어를 떠서 시편을 채취하여 경도, 인장강도, 굴곡강도, 압축응력, 열변형온도 및 흡수율을 측정하였고, 외관을 관찰하였다.After the construction of the resin mortar according to the above embodiment, the specimen was taken from the core by floating the core, and the hardness, tensile strength, flexural strength, compressive stress, heat deformation temperature, and water absorption were measured, and the appearance was observed.

여기서, 경도는 록웰경도로서 그 결과 80∼90(M-scale)이고, 인장강도는 JIS K 6911에 의해 측정하였으며 그 결과 350∼380 ㎏/㎠ 이다.Here, the hardness is Rockwell hardness, the result is 80 ~ 90 (M-scale), the tensile strength was measured according to JIS K 6911 and the result is 350 ~ 380 kg / ㎠.

그리고, 굴곡강도는 ASTM D 790에 의해 측정하였고 그결과 550∼600㎏/㎠이고, 압축응력은 ASTM D 695 방법에 의해 측정하였으며, 그 결과 340∼400㎏/㎠이었다.The flexural strength was measured by ASTM D 790 and as a result was 550-600 kg / cm 2, and the compressive stress was measured by ASTM D 695 method, and the result was 340-400 kg / cm 2.

열변형온도는 ASTM 648에 의해 측정하였고 그 결과는 95℃였으며, 흡수열은 JIS K 6911에 따라 측정하였으며 그 결과 0.2% 이었다.The heat deflection temperature was measured by ASTM 648. The result was 95 ° C., and the heat of absorption was measured according to JIS K 6911. The result was 0.2%.

한편, 외관이 두께가 일정하게 코팅되어 미려하고, 롤러형태에 따라 그 표면의 형태가 변화한다.On the other hand, the appearance is beautifully coated with a uniform thickness, the shape of the surface changes according to the roller shape.

Claims (3)

에폭시 수지를 기본수지로 하고 여기에 경화제, 경화촉진제 및 안료등의 첨가제를 혼합하여 이루어진 에폭시 수지 모르타르를 시공하는 방법에 있어서, 상기 에폭시 수지 모르타르 조성물에 자연석 또는 인조석 규사를 배합하고 포설한 다음 압착미장하고 경화시킨 후, 그 표면층에 응집성 성형코팅재를 일정 두께로 메꾸는 것을 특징으로 하는 에폭시 수지 모르타르 시공방법.In the method of constructing an epoxy resin mortar made of an epoxy resin as a base resin and mixing additives such as a curing agent, a curing accelerator, and a pigment therein, the natural resin or artificial silica sand is added to the epoxy resin mortar composition and laid, followed by compression plastering. And hardening, and then filling the cohesive molding coating material in a predetermined thickness on the surface layer of the epoxy resin mortar. 제1항에 있어서, 상기 응집성 성형코팅재로는 에폭시 수지 70∼80 중량%, 가소제 3∼5 중량%, 치소제 4∼5 중량%, 비반응성 희석재 14∼16 중량% 및 소포제 0.05∼0.1 중량%로 이루어진 주재 100 중량부와 이에 대하여 경화제 50∼60 중량%, 레진 아닥트제 7∼15 중량% 및 촉진제 25∼33 중량%로 이루어진 경화제 50 중량부로 이루어진 조성물을 사용하는 것을 특징으로 하는 에폭시 수지 모르타르 시공방법.According to claim 1, wherein the cohesive molding coating material is 70 to 80% by weight epoxy resin, 3 to 5% by weight plasticizer, 4 to 5% by weight plasticizer, 14 to 16% by weight non-reactive diluent and 0.05 to 0.1 weight defoamer Epoxy resin, characterized by using a composition consisting of 100 parts by weight of a main material composed of% and 50 parts by weight of a curing agent comprising 50 to 60% by weight of a curing agent, 7 to 15% by weight of a resin adduct and 25 to 33% by weight of an accelerator. Mortar construction method. 제1항에 있어서, 상기 응집성 성형코팅재 시공시 트리에틸렌테트라아민 또는 디에틸트리아민 0.5∼1.0 중량%를 혼합하여 사용하는 것을 특징으로하는 에폭시 수지 모르타르 시공방법.The method of claim 1, wherein 0.5 to 1.0% by weight of triethylenetetraamine or diethyltriamine are mixed and used when constructing the cohesive molding coating material.
KR1019960001581A 1996-01-25 1996-01-25 Epoxy resin mortar KR0145117B1 (en)