JPH1159129A - High speed and heavy load retreaded tire - Google Patents

High speed and heavy load retreaded tire

Info

Publication number
JPH1159129A
JPH1159129A JP9228306A JP22830697A JPH1159129A JP H1159129 A JPH1159129 A JP H1159129A JP 9228306 A JP9228306 A JP 9228306A JP 22830697 A JP22830697 A JP 22830697A JP H1159129 A JPH1159129 A JP H1159129A
Authority
JP
Japan
Prior art keywords
layer
tire
rubber
thickness
reinforcing fabric
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP9228306A
Other languages
Japanese (ja)
Inventor
Koji Hayashi
浩司 林
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Bridgestone Corp
Original Assignee
Bridgestone Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Bridgestone Corp filed Critical Bridgestone Corp
Priority to JP9228306A priority Critical patent/JPH1159129A/en
Publication of JPH1159129A publication Critical patent/JPH1159129A/en
Pending legal-status Critical Current

Abstract

PROBLEM TO BE SOLVED: To provide a durable retreaded tire in which retreadability is improved in retreading the tire without giving damage to the cords in the outermost layer of the crown part of a carcass main body of the tire. SOLUTION: In a retreaded tire on which a new tread rubber is stuck, a reinforced fabric layer comprising at least one layer of rubber coated cords is arranged adjacent to the outside of the crown part of the tire. Also the thickness S of the rubber layer formed between the cords in the innermost layer 1 of the reinforced fabric layer and the cords in the outermost layer of the crown part of the carcass main body of the tire is 0.8 to 2.3 times the diameter of the cards D in the innermost layer of the reinforced fabric layer, and the thickness (t) of the coated rubber layer on the outside of the cords in the innermost layer of the reinforced fabric layer is smaller than the thickness of the rubber layer formed between the cords in the innermost layer of the reinforced fabric layer and the cords in the outermost layer of the crown part of the carcass main body of the tire.

Description

【発明の詳細な説明】DETAILED DESCRIPTION OF THE INVENTION

【0001】[0001]

【発明の属する技術分野】本発明は空気入り更生タイヤ
に関するもので、特に、航空機用更生タイヤに代表され
る高速重荷重用更生タイヤに関するものである。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a pneumatic retread tire, and more particularly to a high-speed heavy-load retread tire represented by an aircraft retread tire.

【0002】[0002]

【従来の技術】従来、航空機用タイヤは、トレッド・ゴ
ムが所定量摩耗すると、残存する古くなったトレッド・
ゴムなどがバフされてタイヤから取り除かれ、いわゆる
更生タイヤの台タイヤが製造され、この台タイヤに、新
たにトレッド・ゴム、補強ファブリック層およびクッシ
ョン・ゴムが張り付けられ更生タイヤとして再利用され
ている。更生タイヤが使用されてそのトレッド・ゴムが
所定量摩耗すると、再度残存する古くなったトレッド・
ゴムなどがバフされてタイヤから取り除かれ、新たにト
レッド・ゴムなどが張り付けられて、繰り返し再利用さ
れる。通常、航空機用タイヤは少なくとも5乃至6回は
更生されて再利用される。タイヤが更生される際に、使
用済みタイヤから取り除かれるのは上記のようにトレッ
ド・ゴム、補強ファブリック層およびクッション・ゴム
などで、台タイヤとして残されるのはカーカス本体であ
る。カーカス本体には左右のビード・コアー、カーカス
・プライおよびサイド・ゴム層の外に、ブレーカーを備
えたバイアス・タイヤではブレーカーがラジアル・タイ
ヤではベルト層が含まれる。本明細書において、「台タ
イヤのカーカス本体」とは、ビード・コアー、カーカス
・プライおよびサイド・ゴム層の外に、ブレーカーを備
えたバイアス・タイヤではブレーカーがラジアル・タイ
ヤではベルト層が含まれ、したがって、「台タイヤのカ
ーカス本体のクラウン部最外層のコード」とは、ラジア
ル・タイヤではベルト層の最外層のコードを指し、ブレ
ーカーを備えたバイアス・タイヤではブレーカーの最外
層のコードを指し、また、ブレーカーを備えていないバ
イアス・タイヤではカーカス・プライの最外層のコード
を指す。
2. Description of the Related Art Conventionally, aircraft tires have a problem in that when a predetermined amount of tread rubber is worn, the remaining aged tread rubber remains.
Rubber and other materials are buffed and removed from the tires, producing so-called retread tire base tires, which have been newly reused as retread tires with new tread rubber, reinforcing fabric layers and cushion rubber attached. . When retreaded tires are used and the tread rubber is worn by a predetermined amount, the remaining tread rubber
Rubber and the like are buffed and removed from the tires, and new tread and rubber are attached and reused repeatedly. Typically, aircraft tires are retreaded and reused at least five or six times. When the tire is rehabilitated, the tread rubber, the reinforcing fabric layer and the cushion rubber are removed from the used tire as described above, and the carcass body is left as the base tire. The carcass body includes bead cores, carcass plies, and side rubber layers on the left and right, a breaker for a bias tire having a breaker, and a belt layer for a radial tire. In the present specification, the `` carcass body of the base tire '' includes a bead core, a carcass ply, and a side rubber layer, a breaker for a bias tire having a breaker, and a belt layer for a radial tire. Therefore, the `` cord of the crown outermost layer of the carcass body of the base tire '' refers to the cord of the outermost layer of the belt layer for radial tires, and refers to the cord of the outermost layer of the breaker for bias tires having breakers. In the case of a bias tire without a breaker, it refers to the cord of the outermost layer of the carcass ply.

【0003】[0003]

【発明が解決しようとする課題】上記のクッション・ゴ
ムは、厚さがおよそ0.5mm程度の幅広のシートであ
るから、台タイヤ上に張り付けるときに皺が発生しやす
く、更生タイヤ製造工程の中でもこのシート張り付け工
程は極めて作業性の悪い工程であった。そこで、本発明
の更生タイヤでは、このクッション・ゴムの使用をやめ
て更生性を改良しようとするものである。しかしなが
ら、クッション・ゴムを単純に廃止すると、当然のこと
ながら、補強ファブリック層の内側のゴム層の厚さが薄
くなるので、次回のタイヤ更生のバフ作業のときに、台
タイヤのカーカス本体のクラウン部最外層のコードを傷
つけることがある。一方、補強ファブリック層の内側の
ゴム層の厚さを厚くすると、ヒート・セパレーション故
障が発生しやすくなり、したがって更生タイヤの耐久性
が低下するという欠点があった。
Since the cushion rubber is a wide sheet having a thickness of about 0.5 mm, wrinkles are easily generated when the cushion rubber is stuck on a base tire. Among these, the sheet attaching process was a process with extremely poor workability. Therefore, in the retreaded tire of the present invention, the use of the cushion rubber is stopped to improve the retreadability. However, if the cushion rubber is simply abolished, naturally, the thickness of the rubber layer inside the reinforcing fabric layer becomes thinner. The outermost layer cord may be damaged. On the other hand, when the thickness of the rubber layer inside the reinforcing fabric layer is increased, a heat separation failure is likely to occur, and thus the durability of the retreaded tire is reduced.

【0004】本発明の目的は、台タイヤのカーカス本体
のクラウン部最外層のコードを傷つけることなく、タイ
ヤを更生するときの更生性を改良した、耐久性に優れた
更生タイヤを提供することである。
[0004] It is an object of the present invention to provide a retread tire having improved durability when retreading the tire without damaging the cord of the outermost layer of the crown portion of the carcass body of the base tire and having excellent durability. is there.

【0005】[0005]

【課題を解決するための手段】上記目的を達成するため
に、本発明による更生タイヤは、使用済みタイヤから残
存する古くなったトレッド・ゴムなどがバフされて取り
除かれた台タイヤに、新たにトレッド・ゴムが張り付け
られた更生タイヤにおいて、(1)該台タイヤのクラウ
ン部外側に隣接して、少なくとも1層のゴム被覆コード
層よりなる、補強ファブリック層が配置され、(2)該
補強ファブリック層の最内層のコードの内側の被覆ゴム
層の厚さTが、該補強ファブリック層の最内層のコード
直径Dの0.8乃至2.3倍で、(3)該補強ファブリ
ック層の最内層のコードの外側の被覆ゴム層の厚さtが
内側の被覆ゴム層の厚さTより小さいことを特徴とする
高速重荷重用更生タイヤである。
In order to achieve the above-mentioned object, a retreaded tire according to the present invention is newly added to a base tire in which old tread rubber or the like remaining from used tires is removed by buffing. In a retread tire to which tread rubber is attached, (1) a reinforcing fabric layer comprising at least one rubber-coated cord layer is disposed adjacent to the outside of a crown portion of the base tire, and (2) the reinforcing fabric (3) the innermost layer of the reinforcing fabric layer has a thickness T of 0.8 to 2.3 times the cord diameter D of the innermost layer of the reinforcing fabric layer; The thickness t of the outer coating rubber layer of the cord is smaller than the thickness T of the inner coating rubber layer.

【0006】従来は、トレッド・ゴム、補強ファブリッ
ク層およびクッション・ゴムが台タイヤに張り付けられ
て更生タイヤが製造されていたので、前述のごとくクッ
ション・ゴムを台タイヤ上に張り付けるときに皺が発生
しやすく、更生タイヤ製造工程の中でもこのシート張り
付け工程は極めて作業性の悪い工程であった。
Conventionally, a tread rubber, a reinforcing fabric layer, and a cushion rubber have been attached to a base tire to manufacture a retreaded tire. As described above, wrinkles occur when the cushion rubber is attached to the base tire. The sheet sticking step is a process that is extremely poor in workability even in the process of manufacturing a retreaded tire.

【0007】本発明の更生タイヤでは、このクッション
・ゴムの使用をやめて更生性を改良しようとするもの
で、上記のように、従来クッション・ゴムが配置されて
いた位置に、すなわち台タイヤのクラウン部外側に隣接
して、少なくとも1層のゴム被覆コード層よりなる、補
強ファブリック層が配置されている。そして、この補強
ファブリック層の最内層のコードの内側の被覆ゴム層の
厚さTが、該補強ファブリック層の最内層のコード直径
Dの0.8乃至2.3倍である。上記のゴム層の厚さが
補強ファブリック層の最内層のコード直径の0.8倍よ
り小さくなると、次回のタイヤ更生のバフ作業のとき
に、台タイヤのカーカス本体のクラウン部最外層のコー
ドを傷つけることがある。一方、上記のゴム層の厚さを
補強ファブリック層の最内層のコード直径の2.3倍よ
り厚くすると、ヒート・セパレーション故障が発生しや
すくなり、したがって更生タイヤの耐久性が低下する。
In the retreaded tire of the present invention, the use of the cushion rubber is stopped to improve the retreadability. As described above, the crown rubber of the base tire is located at the position where the cushion rubber is conventionally disposed. Adjacent to the outside is a reinforcing fabric layer comprising at least one rubber-coated cord layer. The thickness T of the rubber coating layer inside the innermost cord of the reinforcing fabric layer is 0.8 to 2.3 times the cord diameter D of the innermost layer of the reinforcing fabric layer. When the thickness of the rubber layer is smaller than 0.8 times the cord diameter of the innermost layer of the reinforcing fabric layer, the cord of the outermost layer of the crown portion of the carcass body of the base tire will be replaced at the next buffing operation of the tire rehabilitation. May hurt. On the other hand, if the thickness of the rubber layer is greater than 2.3 times the cord diameter of the innermost layer of the reinforcing fabric layer, a heat separation failure is likely to occur, and thus the durability of the retreaded tire is reduced.

【0008】本発明の更生タイヤでは、上記のように、
補強ファブリック層の最内層のコードの外側の被覆ゴム
層の厚さtが内側の被覆ゴム層の厚さTより小さいこと
が必要である。これは、補強ファブリック層の最内層の
コードの外側の被覆ゴム層の厚さtが内側の被覆ゴム層
の厚さTより大きいと、ヒート・セパレーション故障が
発生しやすくなり、したがって更生タイヤの耐久性が低
下するからである。
In the retread tire of the present invention, as described above,
It is necessary that the thickness t of the outer coating rubber layer of the innermost cord of the reinforcing fabric layer is smaller than the thickness T of the inner coating rubber layer. This is because if the thickness t of the outer coating rubber layer of the cord of the innermost layer of the reinforcing fabric layer is larger than the thickness T of the inner coating rubber layer, a heat separation failure is likely to occur, and therefore the durability of the retreaded tire is increased. This is because the property is reduced.

【0009】本発明による更生タイヤでは、上記のよう
に、補強ファブリック層の最内層のコード被覆ゴム層の
厚さが内側と外側では異なり、内側のゴム層の厚さが外
側のゴム層の厚さより大きいことが、ヒート・セパレー
ション故障を防止するために好ましい。
In the retread tire according to the present invention, as described above, the thickness of the innermost cord-coated rubber layer of the reinforcing fabric layer is different between the inside and the outside, and the thickness of the inside rubber layer is the thickness of the outside rubber layer. Larger is preferred to prevent heat separation failure.

【0010】[0010]

【発明の実施の形態】以下、本発明に従う実施例のタイ
ヤおよび比較例のタイヤについて図面を参照して説明す
る。いずれもトレッド・ゴムが所定量摩耗し、1回目の
寿命を終了した航空機用空気入りバイアス・タイヤに残
存する古くなったトレッド・ゴムなどをバフして取り除
き新たに補強ファブリック層およびトレッド・ゴムを張
り替えた更生タイヤであって、タイヤ・サイズはH49
×19.0−22 32PRである。
DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, a tire according to an embodiment of the present invention and a tire according to a comparative example will be described with reference to the drawings. In each case, the tread rubber is worn by a predetermined amount and the old tread rubber remaining on the pneumatic bias tire for aircraft whose first life has expired is buffed off and the reinforcing fabric layer and the tread rubber are newly added. This is a rehabilitated retreaded tire with a tire size of H49
× 19.0-22 32PR.

【0011】図1は、実施例のタイヤの補強ファブリッ
ク層の最内層と台タイヤのカーカス本体のクラウン部最
外層との一部断面図である。実施例のタイヤは、トレッ
ド・ゴムが所定量摩耗し、1回目の寿命を終了した航空
機用空気入りバイアス・タイヤに残存する古くなったト
レッド・ゴムなどをバフして取り除き新たに補強ファブ
リック層およびトレッド・ゴムを張り替えた更生タイヤ
であって、台タイヤのクラウン部外側に隣接して1層の
ゴム被覆コード層よりなる、補強ファブリック層が配置
され、補強ファブリック層の最内層1のコードの内側の
被覆ゴム層の厚さT=0.75mmが補強ファブリック
層の最内層のコード直径D=0.51mmの1.47倍
であり、補強ファブリック層の最内層1のコードの外側
の被覆ゴム層の厚さt=0.25mmが内側の被覆ゴム
層の厚さTより小さい。
FIG. 1 is a partial sectional view of the innermost layer of the reinforcing fabric layer of the tire of the embodiment and the outermost layer of the crown portion of the carcass body of the base tire. In the tire of the embodiment, the tread rubber is worn by a predetermined amount, the old tread rubber remaining in the pneumatic bias tire for aircraft which has finished the first life is buffed and removed, and a new reinforcing fabric layer and A retreaded tire in which tread rubber is replaced, wherein a reinforcing fabric layer comprising a rubber-coated cord layer is disposed adjacent to the outside of a crown portion of a base tire, and the inside of a cord of an innermost layer 1 of the reinforcing fabric layer. The thickness T = 0.75 mm of the covering rubber layer is 1.47 times the cord diameter D = 0.51 mm of the innermost layer of the reinforcing fabric layer, and the outer covering rubber layer of the cord of the innermost layer 1 of the reinforcing fabric layer. Is smaller than the thickness T of the inner coating rubber layer.

【0012】比較例のタイヤは、補強ファブリック層の
最内層1のコードの内側の被覆ゴム層の厚さT=0.2
5mmが補強ファブリック層の最内層のコード直径D=
0.51mmの0.49倍であり、補強ファブリック層
の最内層1のコードの外側の被覆ゴム層の厚さt=0.
25mmが内側の被覆ゴム層の厚さTと同じであること
を除いて、上記実施例のタイヤとほぼ同じである。
The tire of the comparative example has a thickness T = 0.2 of the covering rubber layer inside the cord of the innermost layer 1 of the reinforcing fabric layer.
5 mm is the cord diameter D of the innermost layer of the reinforcing fabric layer =
It is 0.49 times of 0.51 mm, and the thickness t = 0.0 of the coating rubber layer outside the cord of the innermost layer 1 of the reinforcing fabric layer.
It is almost the same as the tire of the above embodiment, except that 25 mm is the same as the thickness T of the inner covering rubber layer.

【0013】次に、これらの実施例のタイヤおよび比較
例のタイヤの比較試験を行った。比較試験の結果では、
実施例のタイヤは、バフ時に台タイヤのカーカスのコー
ド露出発生は皆無であったが、比較例のタイヤではバフ
面全体の約15%にコード露出が発生していた。
Next, comparative tests were performed on the tires of these examples and the comparative example. In the results of the comparative test,
In the tire of Example, no cord exposure occurred in the carcass of the base tire at the time of buffing, but in the tire of Comparative Example, cord exposure occurred in about 15% of the entire buff surface.

【0014】上記の比較試験の結果を、実施例のタイヤ
および比較例のタイヤの概要とともに、表1に示す。
The results of the above comparative tests are shown in Table 1 together with the outlines of the tires of the examples and the comparative examples.

【0015】[0015]

【表1】 [Table 1]

【0016】[0016]

【発明の効果】表1に示す比較試験の結果から、実施例
のタイヤは比較例のタイヤに比べ、バフ時に台タイヤの
カーカスのコード露出が発生しない、優れたタイヤであ
ることがわかる。
From the results of the comparative test shown in Table 1, it can be seen that the tire of the example is an excellent tire in which the carcass cord exposure of the base tire does not occur during buffing as compared with the tire of the comparative example.

【図面の簡単な説明】[Brief description of the drawings]

【図1】補強ファブリック層と台タイヤのカーカスの一
部断面図である。
FIG. 1 is a partial cross-sectional view of a reinforcing fabric layer and a carcass of a base tire.

【符号の説明】[Explanation of symbols]

1 補強ファブリック層の最内層 2 台タイヤのカーカス本体のクラウン部最外層 D コード直径 S ゴム層の厚さ t 外側の被覆ゴム層の厚さ T 内側の被覆ゴム層の厚さ 1 Innermost layer of reinforcing fabric layer 2 Outermost layer of crown portion of carcass body of two tires D Code diameter S Thickness of rubber layer t Thickness of outer coating rubber layer T Thickness of inner coating rubber layer

Claims (1)

【特許請求の範囲】[Claims] 【請求項1】 使用済みタイヤから残存する古くなった
トレッド・ゴムなどがバフされて取り除かれた台タイヤ
に、新たにトレッド・ゴムが張り付けられた更生タイヤ
において、(1)該台タイヤのクラウン部外側に隣接し
て、少なくとも1層のゴム被覆コード層よりなる、補強
ファブリック層が配置され、(2)該補強ファブリック
層の最内層のコードの内側の被覆ゴム層の厚さTが、該
補強ファブリック層の最内層のコード直径Dの0.8至
2.3倍で、(3)該補強ファブリック層の最内層のコ
ードの外側の被覆ゴム層の厚さtが内側の被覆ゴム層の
厚さTより小さいことを特徴とする高速重荷重用更生タ
イヤ。
1. A retreaded tire in which tread rubber is newly attached to a base tire from which old tread rubber or the like remaining from used tires has been buffed and removed, and (1) a crown of the base tire A reinforcing fabric layer comprising at least one rubber-coated cord layer is disposed adjacent to the outer side, and (2) the thickness T of the coating rubber layer inside the innermost cord of the reinforcing fabric layer is such that 0.8 to 2.3 times the cord diameter D of the innermost layer of the reinforcing fabric layer, and (3) the thickness t of the outer covering rubber layer of the innermost cord of the reinforcing fabric layer is smaller than that of the inner covering rubber layer. A high-speed heavy-load retreaded tire having a thickness smaller than T.
JP9228306A 1997-08-25 1997-08-25 High speed and heavy load retreaded tire Pending JPH1159129A (en)