JPH05163684A - Production of leathery sheet-like product - Google Patents
Production of leathery sheet-like productInfo
- Publication number
- JPH05163684A JPH05163684A JP3350768A JP35076891A JPH05163684A JP H05163684 A JPH05163684 A JP H05163684A JP 3350768 A JP3350768 A JP 3350768A JP 35076891 A JP35076891 A JP 35076891A JP H05163684 A JPH05163684 A JP H05163684A
- Authority
- JP
- Japan
- Prior art keywords
- polyurethane
- parts
- leather
- polycarbonate
- sheet
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Withdrawn
Abstract
Description
【0001】[0001]
【産業上の利用分野】本発明は、皮革様シート状物の製
造方法に関し、さらに詳しくは家具用材料、車両用内
装、シート材料などに好適な難燃性に優れた皮革様シー
ト状物の製造方法に関する。BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a method for producing a leather-like sheet material, and more particularly, a leather-like sheet material having excellent flame retardancy suitable for furniture materials, vehicle interiors, sheet materials and the like. It relates to a manufacturing method.
【0002】[0002]
【従来の技術】家具用材料、車両用材料、特に車両内装
材料については、火災時の人的被害を防止するため、近
年、難燃化が強く要求されるようになってきており、例
えば自動車内装材については、米国難燃規格のFMVS
S−302や我が国のJIS−D−1201などが規定
され、これらの規定に合格することが要求される。2. Description of the Related Art In recent years, there has been a strong demand for flame retardancy in furniture materials, vehicle materials, and in particular vehicle interior materials in order to prevent human damage in the event of a fire. For interior materials, FMVS of American flame retardant standard
S-302 and Japanese JIS-D-1201, etc. are specified, and it is required to pass these rules.
【0003】ポリカーボネート系ポリウレタンは、耐加
水分解性、耐光性に優れ、皮革用シート材料として前記
用途に好適であることが知られている。従来、該ポリウ
レタンの湿式凝固法による皮革様シート状物の難燃化方
法としては、難燃剤として、トリクレジルホスフェート
などのリン酸エステル系化合物を配合する方法が知られ
ている。Polycarbonate polyurethane is known to be excellent in hydrolysis resistance and light resistance and suitable for the above-mentioned applications as a leather sheet material. Conventionally, as a method of making a leather-like sheet material flame-retardant by a wet coagulation method of the polyurethane, a method of blending a phosphate ester compound such as tricresyl phosphate as a flame retardant is known.
【0004】しかし、リン酸エステル系難燃剤は、湿式
凝固処理中に水中に溶出してその効果が低下すること、
該ポリウレタンの成膜性能または凝固性能を著しく低下
させるという問題があり、さらにはスポンジ構造物を得
ようとする場合に均一なスポンジ構造物が得難く、また
風合いの劣るものしか得られないという欠点がある。However, the phosphoric acid ester type flame retardant is liable to be dissolved in water during the wet coagulation treatment to reduce its effect.
There is a problem that the film forming performance or the coagulation performance of the polyurethane is remarkably lowered, and further, when obtaining a sponge structure, it is difficult to obtain a uniform sponge structure and only a poor texture is obtained. There is.
【0005】[0005]
【発明が解決しようとする課題】本発明は、湿式凝固
性、外観、風合いを損なうことなく、難燃性に優れた皮
革様シート状物の製造方法を提供することを目的とす
る。SUMMARY OF THE INVENTION It is an object of the present invention to provide a method for producing a leather-like sheet material excellent in flame retardancy without impairing wet coagulation properties, appearance and texture.
【0006】[0006]
【課題を解決するための手段】本発明は、ポリカーボネ
ート系ポリウレタン100重量部に対して赤リン系難燃
剤5〜40重量部を含有するポリカーボネート系ポリウ
レタンの溶剤溶液を繊維基材に含浸、および/または塗
布したのち、該ポリウレタンの非溶剤で凝固させて繊維
基材上にポリウレタンの多孔質膜を形成させ、次いで該
多孔質膜表面に表皮層を設けることを特徴とする皮革様
シート状物の製造方法である。According to the present invention, a fiber base material is impregnated with a solvent solution of a polycarbonate polyurethane containing 5 to 40 parts by weight of a red phosphorus flame retardant per 100 parts by weight of a polycarbonate polyurethane, and / or Alternatively, after coating, the polyurethane-like solvent is coagulated with a non-solvent to form a polyurethane porous film on a fiber substrate, and then a skin layer is provided on the surface of the porous film. It is a manufacturing method.
【0007】本発明において、ポリカーボネート系ポリ
ウレタンとは、ポリカーボネート系ポリオールと有機ジ
イソシアネートおよび鎖伸長剤との重合物をいい、ポリ
カーボネート系ポリオールとは、一般式 HO−R−(O−CO−O−R)n −OH 〔ただし、式中、R=−(CH2 )m −、m≧2、n=
5〜200である〕で表されるポリアルキレンポリカー
ボネート系ポリオールであり、具体的には、1,6−ヘ
キサンポリカーボネートポリオールが好ましい。また、
前記ポリアルキレンポリカーボネート系ポリオールの一
部を必要に応じてポリオキシアルキレン変性ポリカーボ
ネートで置換した混合物なども使用できる。In the present invention, the polycarbonate-based polyurethane means a polymer of a polycarbonate-based polyol, an organic diisocyanate and a chain extender, and the polycarbonate-based polyol means a general formula HO-R- (O-CO-O-R). ) n -OH [in the formula, R = - (CH 2) m -, m ≧ 2, n =
5 to 200]. Specifically, 1,6-hexane polycarbonate polyol is preferable. Also,
A mixture obtained by substituting a part of the polyalkylene polycarbonate-based polyol with a polyoxyalkylene-modified polycarbonate can also be used.
【0008】一方、有機ジイソシアネートとしては、無
黄変型ジイソシアネートとして脂肪族もしくは脂環族の
ジイソシアネートが好ましく、例えばテトラメチレンジ
イソシアネート、1,6−ヘキサンジイソシアネート、
2,2,4−トリメチル−1,6−ヘキサンジイソシア
ネート、1−メチルシクロヘキサン−2,4−ジイソシ
アネート、3,3′−ジメチル−4,4′−ジイソシア
ネートジシクロヘキシルメタン、4,4′−ジシクロヘ
キシルメタンジイソシアネートが挙げられる。On the other hand, as the organic diisocyanate, an aliphatic or alicyclic diisocyanate is preferable as the non-yellowing type diisocyanate, for example, tetramethylene diisocyanate, 1,6-hexane diisocyanate,
2,2,4-Trimethyl-1,6-hexanediisocyanate, 1-methylcyclohexane-2,4-diisocyanate, 3,3'-dimethyl-4,4'-diisocyanate dicyclohexylmethane, 4,4'-dicyclohexylmethane diisocyanate Is mentioned.
【0009】さらに、黄変型ジイソシアネートとして、
芳香族ジイソシアネート、例えばトリレンジイソシアネ
ート、ジフェニルメタンジイソシアネート、キシリレン
ジイソシアネートなどを使用することができる。Further, as a yellowing diisocyanate,
Aromatic diisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate and the like can be used.
【0010】また、鎖伸長剤としては、第1級または第
2級の脂肪族アミンあるいは低分子グリコールであっ
て、ピペラジン、ヘキサメチレンジアミン、エチレンジ
アミン、プロピレン−1,2−ジアミン、N−メチル−
ビス−(3−アミノプロピル)アミン、1,4−ジアミ
ノシクロヘキサン、1−アミノ−3−アミノメチル−
3,5,5−トリメチル−シクロヘキサン、1,4−ブ
タンジオール、エチレングリコール、1,6−ヘキサン
ジオール、ネオペンチルグリコール、p−キシリレング
リコールなどが使用できる。The chain extender may be a primary or secondary aliphatic amine or a low molecular weight glycol, such as piperazine, hexamethylenediamine, ethylenediamine, propylene-1,2-diamine, N-methyl-.
Bis- (3-aminopropyl) amine, 1,4-diaminocyclohexane, 1-amino-3-aminomethyl-
3,5,5-Trimethyl-cyclohexane, 1,4-butanediol, ethylene glycol, 1,6-hexanediol, neopentyl glycol, p-xylylene glycol and the like can be used.
【0011】ポリウレタン中には、必要に応じて、成膜
助剤、着色剤、充填剤、光安定剤、紫外線吸収剤、酸化
防止剤、撥水撥油剤などの各種添加剤を混入することが
できる。If necessary, various additives such as film-forming aids, colorants, fillers, light stabilizers, ultraviolet absorbers, antioxidants, and water / oil repellents may be mixed in the polyurethane. it can.
【0012】赤リン系難燃剤としては、混練作業中の発
火を防止するため粒子表面を樹脂で被覆されるなどの処
理を施されたものが好ましく、かかる赤リン系難燃剤と
しては、例えばノーバレッド、ノーバエクセル、ノーバ
ゾール、ノーバクエル〔いずれも燐化学工業(株)
製〕、ヒシガード〔日本化学工業(株)製〕などを挙げ
ることができる。The red phosphorus-based flame retardant is preferably one whose surface is coated with a resin in order to prevent ignition during kneading, and such red phosphorus-based flame retardant is, for example, NOVA. Red, Nova Excel, Novazol, Novaquell [all are Rin Kagaku Co., Ltd.
Manufactured by Nippon Chemical Industry Co., Ltd., and the like.
【0013】赤リン系難燃剤は、従来のリン酸エステル
系難燃剤のように湿式凝固処理中に水中に溶出したり、
ポリウレタンの凝固、成膜性に悪影響を及ぼすことがな
く、またポリウレタンとの親和性が良好なため、混練が
容易であり、凝集せず、長時間均質な分散状態を維持し
沈降しがたいという特徴を有する。また、得られる皮革
状物の外観、風合い、物性を損なうことがなく、さらに
は例え燃焼しても従来の難燃剤に比較して低発煙性であ
り、ドリップ現象もみられない。The red phosphorus flame retardant is eluted in water during the wet coagulation treatment like conventional phosphoric acid ester flame retardants,
Since it does not adversely affect the coagulation and film-forming properties of polyurethane and has good affinity with polyurethane, it is easy to knead, does not aggregate, maintains a homogeneous dispersed state for a long time, and is unlikely to sediment. It has characteristics. Further, the appearance, texture, and physical properties of the obtained leather-like material are not impaired, and even if it burns, it has lower smoke emission compared to conventional flame retardants and no drip phenomenon is observed.
【0014】本発明において、前記難燃剤は、ポリカー
ボネート系ポリウレタン100重量部に対し、5〜40
重量部、好ましくは8〜25重量部添加する。該添加量
が5重量部未満では難燃効果が発揮されず、一方40重
量部を超えると難燃効果は飽和し、赤リン本来の着色が
著しくなり好ましくない。In the present invention, the flame retardant is 5 to 40 parts by weight based on 100 parts by weight of the polycarbonate polyurethane.
Add parts by weight, preferably 8 to 25 parts by weight. If the amount added is less than 5 parts by weight, the flame retardant effect will not be exhibited, while if it exceeds 40 parts by weight, the flame retardant effect will be saturated and the original coloring of red phosphorus will be remarkable, such being undesirable.
【0015】ポリカーボネート系ポリウレタンの溶剤と
しては、ジメチルホルムアミド、ジメチルアセトアミ
ド、ジメチルスルフォキシド、テトラヒドロフランなど
の有機溶剤を用いることができる。As a solvent for the polycarbonate polyurethane, an organic solvent such as dimethylformamide, dimethylacetamide, dimethylsulfoxide and tetrahydrofuran can be used.
【0016】本発明においては、前記ポリカーボネート
系ポリウレタン、規定量の赤リン系難燃剤を前記溶剤に
溶解および分散させて得られたポリウレタン溶液(以下
「ポリウレタン組成液」という)を繊維基材に含浸およ
び/または塗布したのち、該ポリウレタンの非溶剤で凝
固させて繊維基材上にポリウレタンの多孔質膜を形成さ
せる。In the present invention, a fiber base material is impregnated with a polyurethane solution (hereinafter referred to as "polyurethane composition liquid") obtained by dissolving and dispersing the polycarbonate polyurethane and a specified amount of the red phosphorus flame retardant in the solvent. After coating and / or coating, the polyurethane is solidified with a non-solvent to form a polyurethane porous film on the fiber substrate.
【0017】前記ポリウレタン組成液には、得られる皮
革様シート状物に形成される湿式セルを微細孔とするた
めの凝固調整剤として、一般に効果があるとされている
ノニオン系界面活性剤を添加することができる。A nonionic surfactant, which is generally considered to be effective, is added to the above-mentioned polyurethane composition liquid as a coagulation regulator for forming fine cells in the wet cells formed in the obtained leather-like sheet. can do.
【0018】本発明において、繊維基材としては、綿、
麻などの天然繊維;レーヨンなどの再生繊維;アセテー
トなどの半合成繊維;ポリアミド、ポリエステル、ポリ
アクリロニトリルなどの合成繊維の単独またはこれらの
混紡繊維よりなる編布、織布、不織布のいずれも用いる
ことができる。なお、繊維基材としては、難燃化処理を
施されたもの、あるいは難燃化された繊維からなる基材
を使用することもできる。かかる繊維基材を用いること
により、さらに優れた難燃性を得ることができる。ま
た、これらの繊維基材は、少なくともポリウレタン組成
液を含浸および/または塗布される面が起毛または立毛
加工を施されたものが好ましい。In the present invention, the fiber base material is cotton,
Natural fibers such as hemp; regenerated fibers such as rayon; semi-synthetic fibers such as acetate; synthetic fibers such as polyamide, polyester, polyacrylonitrile, etc., either alone or as a knitted fabric, woven fabric or non-woven fabric made of a blend of these fibers You can As the fiber base material, it is possible to use a base material that has been subjected to a flame-retardant treatment, or a base material that is made of flame-retarded fiber. By using such a fiber base material, more excellent flame retardancy can be obtained. In addition, it is preferable that at least the surface of the fiber base material, which is impregnated and / or coated with the polyurethane composition liquid, has been raised or napped.
【0019】本発明においては、まず前記繊維基材にポ
リウレタン組成液を含浸、および/または塗布する。ポ
リウレタン組成液の塗布はナイフコーター、リバーウロ
ールコーターなどにより行うことができる。ポリウレタ
ン組成液の含浸および/または塗布の量は、対繊維重量
あたりポリウレタン固形分換算で10〜200重量%、
好ましくは20〜100重量%程度である。In the present invention, first, the fiber base material is impregnated with and / or coated with a polyurethane composition liquid. The polyurethane composition liquid can be applied by a knife coater, a river roll coater, or the like. The amount of the polyurethane composition liquid impregnated and / or applied is 10 to 200% by weight in terms of polyurethane solid content per weight of fiber,
It is preferably about 20 to 100% by weight.
【0020】次に、ポリウレタン組成液を含浸および/
または塗布された繊維基材を、ポリウレタンの非溶剤で
処理しポリウレタンを凝固させる。ポリウレタンの非溶
剤としては、例えば、水、水とジメチルホルムアミドと
の混合溶媒を用いることができる。かかる非溶剤による
処理は、例えばポリウレタン組成液を含浸および/また
は塗布した繊維基材を15〜60℃の水中に3〜60分
間浸漬することにより行うことができ、さらに温水中で
洗浄を繰り返して脱溶媒し、脱水乾燥することにより、
繊維基材上に微細孔を有するポリウレタンの多孔質膜を
形成させることができる。Next, the polyurethane composition liquid is impregnated and / or
Alternatively, the coated fiber substrate is treated with a nonsolvent for polyurethane to solidify the polyurethane. As the non-solvent for polyurethane, for example, water or a mixed solvent of water and dimethylformamide can be used. The treatment with such a non-solvent can be performed, for example, by immersing the fiber base material impregnated and / or coated with the polyurethane composition liquid in water at 15 to 60 ° C. for 3 to 60 minutes, and further repeating the washing in warm water to repeat the washing. By removing the solvent and dehydrating and drying,
It is possible to form a polyurethane porous film having fine pores on a fiber substrate.
【0021】ポリウレタンの多孔質膜は、100%モジ
ュラスが20〜120kg/cm2 であることが好まし
い。100%モジュラスが20kg/cm2 未満では風
合いはソフトになるが物性が劣り実用的でなく、一方1
20kg/cm2 を超えると物性は向上するが風合いが
ハードになって好ましくない。The porous polyurethane membrane preferably has a 100% modulus of 20 to 120 kg / cm 2 . When the 100% modulus is less than 20 kg / cm 2 , the texture becomes soft, but the physical properties are inferior and not practical. On the other hand, 1
If it exceeds 20 kg / cm 2 , the physical properties are improved, but the texture becomes hard, which is not preferable.
【0022】本発明においては、次に、繊維基材上に形
成されたポリウレタンの多孔質膜の表面に表皮層を設け
て皮革様シート状物を得る。表皮層としては、ポリウレ
タン樹脂から構成された、厚さ5〜100μmの膜が好
ましい。表皮層用のポリウレタン樹脂としては、ポリエ
ステル系ポリウレタン、ポリエーテル系ポリウレタン、
ポリカプロラクトン系ポリウレタン、ポリメチルバレロ
ラクトン系ポリウレタン、ポリカーボネート系ポリウレ
タンなどのいずれも使用可能であるが、なかでもポリカ
ーボネート系ポリウレタンが耐久性、耐熱性に富み、好
ましい。In the present invention, a leather-like sheet material is then obtained by providing a surface skin layer on the surface of the porous polyurethane membrane formed on the fiber base material. As the skin layer, a film made of polyurethane resin and having a thickness of 5 to 100 μm is preferable. As the polyurethane resin for the skin layer, polyester-based polyurethane, polyether-based polyurethane,
Any of polycaprolactone-based polyurethane, polymethylvalerolactone-based polyurethane, polycarbonate-based polyurethane and the like can be used. Among them, polycarbonate-based polyurethane is preferable because it has excellent durability and heat resistance.
【0023】また、表皮層を形成するポリウレタン樹脂
膜としては、100%モジュラスが30〜200kg/
cm2 のものが好ましい。100%モジュラスが30k
g/cm2 未満では風合いはソフトになるが表面強度が
劣り、一方200kg/cm2 を超えると風合いがハー
ドになって好ましくない。The polyurethane resin film forming the skin layer has a 100% modulus of 30 to 200 kg /
cm 2 is preferable. 100% modulus is 30k
If it is less than g / cm 2 , the texture will be soft, but the surface strength will be poor, while if it exceeds 200 kg / cm 2 , the texture will be hard, which is not preferable.
【0024】本発明において、表皮層の形成は、例えば
離型紙に表皮層形成用樹脂を塗布、乾燥させたのち、該
離型紙を繊維基材上に形成されたポリウレタンの多孔質
膜の表面に熱ラミネートし、しかる後、離型紙を剥離す
る転写法によって積層して行うことができる。また、表
皮層を構成するためのポリウレタンの溶剤溶液を多孔質
膜の表面に直接塗布する方法によることもできる。表皮
層の形成は、接着剤を介してまたは介すことなく行う。In the present invention, the skin layer is formed by, for example, applying a skin layer-forming resin to a release paper and drying the release paper, and then applying the release paper to the surface of a porous polyurethane membrane formed on a fiber substrate. It can be carried out by heat laminating, and then laminating by a transfer method in which the release paper is peeled off. Alternatively, a method in which a solvent solution of polyurethane for forming the skin layer is directly applied to the surface of the porous membrane can be used. The skin layer is formed with or without an adhesive.
【0025】接着剤を用いる場合は、得られる皮革様シ
ート状物の難燃性を向上させるため接着剤は、その中に
赤リン系難燃剤を、前記と同様の理由から、ポリウレタ
ン100重量部に対し5〜40重量部含有することが好
ましい。難燃剤の量はさらに好ましくは8〜25重量部
である。When an adhesive is used, in order to improve the flame retardancy of the obtained leather-like sheet material, the adhesive contains a red phosphorus flame retardant therein, and for the same reason as above, 100 parts by weight of polyurethane. However, it is preferable to contain 5 to 40 parts by weight. The amount of flame retardant is more preferably 8 to 25 parts by weight.
【0026】用いられる接着剤としては、例えばポリエ
ステル系ポリウレタン、ポリエーテル系ポリウレタン、
ポリカプロラクトン系ポリウレタン、ポリメチルバレロ
ラクトン系ポリウレタン、ポリカーボネート系ポリウレ
タンなどの2液型ポリウレタン樹脂を挙げることができ
る。なかでも耐久性、耐熱性の観点からポリカーボネー
ト系ポリウレタンの2液型接着剤が好ましい。Examples of the adhesive used include polyester polyurethane, polyether polyurethane,
Two-component polyurethane resins such as polycaprolactone-based polyurethane, polymethylvalerolactone-based polyurethane and polycarbonate-based polyurethane can be mentioned. Among them, a polycarbonate polyurethane two-component adhesive is preferable from the viewpoint of durability and heat resistance.
【0027】本発明により得られる皮革様シート状物の
層構成としては、工程を加味した断面模式図を用いて説
明すると、例えば図1に示すような、繊維基材にポリウ
レタン組成液を含浸凝固させて形成されたポリウレタン
多孔質膜21の表面に接着層30を介して表皮層40が
設けられたもの、図2に示すような、繊維基材にポリウ
レタン組成液を含浸凝固させて形成されたポリウレタン
多孔質膜21に接してさらに同組成液を塗布後凝固させ
て形成されたポリウレタン多孔質膜22の表面に接着層
30を介して表皮層40が設けられたもの、図3に示す
ような、繊維基材10にポリウレタン組成液を塗布凝固
させて繊維基材表面に形成されたポリウレタン多孔質膜
22の表面に接着層30を介して表皮層40が設けられ
た構成のものなどを挙げることができる。The layer structure of the leather-like sheet material obtained by the present invention will be described with reference to a schematic sectional view in which the steps are taken into consideration. For example, as shown in FIG. 1, a fiber base material is impregnated with a polyurethane composition liquid and solidified. The surface of the polyurethane porous membrane 21 thus formed is provided with the skin layer 40 via the adhesive layer 30, and is formed by impregnating and solidifying a polyurethane composition liquid into a fiber base material as shown in FIG. A surface layer 40 is provided on the surface of a polyurethane porous film 22 formed by coating the same composition liquid in contact with the polyurethane porous film 21 and then solidifying the same, as shown in FIG. A structure in which the skin layer 40 is provided on the surface of the polyurethane porous film 22 formed on the surface of the fiber base material by coating and coagulating the polyurethane composition liquid on the fiber base material 10 with the adhesive layer 30 interposed therebetween. It can be mentioned.
【0028】[0028]
【実施例】以下に実施例を挙げて本発明をさらに詳細に
説明するが、本発明はこれらの実施例に限定されるもの
ではない。なお、実施例中、部は重量部を表す。 実施例1 1,6−ヘキサンカーボネートポリオールを主成分とす
る100%モジュラスが35kg/cm2 の難黄変型ポ
リウレタン〔製品名:クリスボンMP−120、大日本
インキ化学工業(株)製〕の16%ジメチルホルムアミ
ド溶液に、ポリウレタン固形分100部あたり、スルホ
コハク酸ジ−2−エチルヘキシルエステルナトリウム塩
4部、ポリエーテル変性シリコンオイル7部、黒色着色
剤5部および赤リン系難燃剤〔製品名:ノーバゾールR
−20、燐化学工業(株)製〕23部を添加してポリウ
レタン組成液を調製した。The present invention will be described in more detail with reference to the following examples, but the present invention is not limited to these examples. In addition, a part represents a weight part in an Example. Example 1 16% of a non-yellowing type polyurethane [Product name: Crisbon MP-120, manufactured by Dainippon Ink and Chemicals, Inc.] containing 1,6-hexane carbonate polyol as a main component and having a 100% modulus of 35 kg / cm 2. To 100 parts of polyurethane solid content in dimethylformamide solution, 4 parts of sodium salt of di-2-ethylhexyl sulfosuccinate, 7 parts of polyether modified silicone oil, 5 parts of black colorant and red phosphorus flame retardant [Product name: Novazol R
-20, manufactured by Rin Kagaku Kogyo Co., Ltd.] 23 parts was added to prepare a polyurethane composition liquid.
【0029】このポリウレタン組成液をポリエステル繊
維とレーヨン繊維を混紡して綾織りに織成した厚み0.
8mmの片面起毛布の含水率70%の起毛面上にナイフ
コーターにて塗布量がポリウレタン固形分で110g/
m2 となるように塗布し、次いで基体をジメチルホルム
アミド11%水溶液(液温度20℃)中に浸漬して凝固
させた。得られたポリウレタンの基体をさらに60℃の
温水中で脱溶媒、洗浄し、乾燥させてポリウレタン多孔
質膜を有するシート状物を得た。該シート状物は、厚み
0.95mmで、表面に均質で微細な空孔を持ったスポ
ンジ構造を有し、柔軟にして面平滑性に優れるものであ
った。This polyurethane composition liquid was twilled and woven by mixing polyester fibers and rayon fibers in a thickness of 0.
On a brushed surface with a water content of 70% of a 8 mm single-sided brushed cloth, a coating amount of 110 g / polyurethane solid content was applied with a knife coater.
m 2 was applied, and then the substrate was immersed in an 11% aqueous solution of dimethylformamide (liquid temperature 20 ° C.) to solidify. The obtained polyurethane substrate was further desolvated in warm water of 60 ° C., washed, and dried to obtain a sheet-shaped product having a polyurethane porous membrane. The sheet-like material had a thickness of 0.95 mm, had a sponge structure with uniform and fine pores on the surface, and was flexible and excellent in surface smoothness.
【0030】次に、シボ付離型紙の表面に、黒色着色剤
20部を含む無黄変型ポリカーボネート系ポリウレタン
樹脂膜、ポリカーボネート系2液型ポリウレタン接着剤
〔架橋剤10部、赤リン系難燃剤:ノーバゾールR−2
0、燐化学工業(株)製、20部を含有〕の層を順次積
層させた離型紙を用いて、転写法により、ポリウレタン
多孔質膜を有するシート状物の表面に該接着剤層を介し
て、無黄変型ポリカーボネート系ポリウレタン樹脂膜を
積層させて、厚さ20μmの表皮層を形成させ、銀付調
皮革様シート状物を得た。得られた皮革様シート状物は
自然な細かい折れしわが発生し、天然皮革に酷似した銀
付外観を有しており、かつ柔軟でボリューム感に富んだ
風合いを持っていた。また、この皮革様シート状物は耐
加水分解性、耐光性、難燃性に優れ、家具、車両用素材
として使用可能であった。Next, on the surface of the embossed release paper, a yellowing-free type polycarbonate-based polyurethane resin film containing 20 parts of a black colorant, a polycarbonate-based two-component polyurethane adhesive [crosslinking agent: 10 parts, red phosphorus-based flame retardant: Novazole R-2
0, manufactured by Rin Kagaku Kogyo Co., Ltd., containing 20 parts] is laminated by a transfer method on the surface of a sheet-like material having a polyurethane porous film through the adhesive layer by a transfer method. Then, a non-yellowing type polycarbonate-based polyurethane resin film was laminated to form a skin layer having a thickness of 20 μm to obtain a silver-tone leather-like sheet. The leather-like sheet obtained had natural fine folds and wrinkles, had a silver-like appearance that was very similar to natural leather, and had a soft and voluminous texture. Moreover, this leather-like sheet was excellent in hydrolysis resistance, light resistance, and flame retardancy, and could be used as a material for furniture and vehicles.
【0031】なお、この皮革様シート状物は、温度70
℃、湿度95%の雰囲気中で10週間ジャングルテスト
をしたのちの、およびフェードメーター(ブラックパネ
ル温度83℃)で200時間照射したのちの外観、風合
い、表面摩耗および剥離強度などの物性の変化は少なか
った。また、FMVSS−302規格による難燃性(燃
焼速度)は42mm/分であった。The leather-like sheet material has a temperature of 70.
Changes in physical properties such as appearance, texture, surface abrasion and peel strength after jungle test for 10 weeks in an atmosphere of ℃ and 95% humidity and after 200 hours of irradiation with a fade meter (black panel temperature 83 ℃) There were few. The flame retardancy (combustion rate) according to the FMVSS-302 standard was 42 mm / min.
【0032】実施例2 1,6−ヘキサンカーボネートポリオールを主成分とす
る100%モジュラスが30kg/cm2 の難黄変型ポ
リウレタン〔製品名:レザミンCu−9430NL、大
日精化工業(株)製〕の10%ジメチルホルムアミド溶
液に、ポリウレタン固形分100部あたり、スルホコハ
ク酸ジ−2−エチルヘキシルエステルナトリウム塩3
部、ポリエチレンオキサイド変性ポリシロキサン4部、
黒色着色剤10部および赤リン系難燃剤〔製品名:ノー
バレッド120UF、燐化学工業(株)製〕18部を添
加してポリウレタン組成液を調製した。Example 2 A non-yellowing type polyurethane [Product name: Resamine Cu-9430NL, manufactured by Dainichiseika Kogyo Co., Ltd.] containing 100% 1,30-hexane carbonate polyol as a main component and having a 100% modulus of 30 kg / cm 2 . 3% sulfosuccinic acid di-2-ethylhexyl ester sodium salt per 100 parts of polyurethane solid content in a 10% dimethylformamide solution
Part, polyethylene oxide modified polysiloxane 4 parts,
A polyurethane composition liquid was prepared by adding 10 parts of a black colorant and 18 parts of a red phosphorus flame retardant [Product name: Nova Red 120UF, manufactured by Rin Kagaku Kogyo KK].
【0033】このポリウレタン組成液を0.2デニール
のポリエステル繊維とナイロン繊維からなる目付250
g/m2 の絡合不織布に、ポリウレタン固形分で75g
/m2 となるように含浸、飽充させた。さらに該繊維基
材上に、1,6−ヘキサンカーボネートポリオールを主
成分とする100%モジュラス50kg/cm2 の難黄
変型ポリウレタン〔製品名:レザミンCu−9450N
L、大日精化工業(株)製〕の17%ジメチルホルムア
ミド溶液に、ポリウレタン固形分100部あたり、1.
5部のスルホコハク酸ジ−2−エチルヘキシルエステル
ナトリウム塩、4部のソルビタンオレイン酸エステル、
10部の黒色着色剤および20部の赤リン系難燃剤〔製
品名:ノーバレッド120UF、燐化学工業(株)製〕
を添加して調製したポリウレタン組成液をナイフコータ
ーにて塗布量が、ポリウレタン固形分で100g/m2
となるように塗布し、次いで基体をジメチルホルムアミ
ド13%溶液(液温度20℃)中に浸漬してポリウレタ
ンを凝固させてポリウレタンの基体を得た。A weight per unit area of 250 denier of polyester resin and nylon fiber was applied to this polyurethane composition liquid.
75 g of polyurethane solid content in g / m 2 entangled nonwoven fabric
It was impregnated so that it would be / m 2, and it was filled up. Further, on the fiber substrate, a yellowing-resistant polyurethane [Product name: Resamine Cu-9450N] containing 100% modulus 50 kg / cm 2 containing 1,6-hexane carbonate polyol as a main component.
L, manufactured by Dainichiseika Kogyo Co., Ltd.] in 17% dimethylformamide solution per 100 parts of polyurethane solid content.
5 parts sulfosuccinic acid di-2-ethylhexyl ester sodium salt, 4 parts sorbitan oleic acid ester,
10 parts of black colorant and 20 parts of red phosphorus flame retardant [Product name: Nova Red 120UF, manufactured by Rin Kagaku Kogyo Co., Ltd.]
The polyurethane composition liquid prepared by adding the above was coated with a knife coater at a coating amount of 100 g / m 2 in terms of polyurethane solid content.
And then the substrate was dipped in a 13% dimethylformamide solution (liquid temperature 20 ° C.) to solidify the polyurethane to obtain a polyurethane substrate.
【0034】得られたポリウレタンの基体をさらに60
℃の温水中で脱溶媒、洗浄し、乾燥させてポリウレタン
多孔質膜を有するシート状物を得た。該シート状物は、
厚さ1.1mmで、表面に均質で微細な空孔を持ったス
ポンジ構造を有し、柔軟にして面平滑性に優れるもので
あった。The resulting polyurethane substrate is further treated with 60
The solvent was removed in warm water of ℃, washed, and dried to obtain a sheet-like material having a polyurethane porous membrane. The sheet is
It had a thickness of 1.1 mm, had a sponge structure with uniform and fine pores on the surface, and was flexible and had excellent surface smoothness.
【0035】このシート状物の表面に実施例1と同様に
して、ポリカーボネート系2液型ポリウレタン接着剤
(架橋剤10部、黒色着色剤10部、および赤リン系難
燃剤:ノーバレッド120UF20部を含有)を介し
て、黒色着色剤20部を含む無黄変型ポリカーボネート
系ポリウレタン樹脂膜を、シボ付離型紙を用いた転写法
により積層させて表皮層を形成させ、銀付調皮革様シー
ト状物に仕上げた。得られた皮革様シート状物は自然な
細かい折れしわが発生し、天然皮革に酷似した銀付外観
を有しており、柔軟性に富んだ風合いを持っていた。ま
たこの皮革様シート状物は耐加水分解性、耐光性、難燃
性に優れ、家具、車両用素材として使用可能であった。In the same manner as in Example 1, a polycarbonate-based two-component polyurethane adhesive (10 parts of a cross-linking agent, 10 parts of a black colorant, and 20 parts of a red phosphorus flame retardant: Novarred 120UF) was applied to the surface of this sheet-like material. A non-yellowing type polycarbonate-based polyurethane resin film containing 20 parts of a black colorant by a transfer method using a textured release paper to form a skin layer, and a silver-finished leather-like sheet material. Finished. The leather-like sheet thus obtained had natural fine folds and wrinkles, had a silver-like appearance that was very similar to natural leather, and had a highly flexible texture. Further, this leather-like sheet was excellent in hydrolysis resistance, light resistance and flame retardancy, and could be used as a material for furniture and vehicles.
【0036】なお、このシート状物は、温度70℃、湿
度95%の雰囲気中で10週間ジャングルテストをした
のちの、およびフェードメーター(ブラックパネル温度
83℃)で200時間照射したのちの、外観、風合い、
表面摩耗性、剥離強度などの物性の変化は少なかった。
また、FMVSS−302規格による難燃性(燃焼速
度)は38mm/分であった。The appearance of this sheet-like material after a jungle test for 10 weeks in an atmosphere at a temperature of 70 ° C. and a humidity of 95% and after irradiation for 200 hours with a fade meter (black panel temperature 83 ° C.) , Texture,
There were few changes in physical properties such as surface wear and peel strength.
The flame retardancy (combustion rate) according to the FMVSS-302 standard was 38 mm / min.
【0037】比較例1 難燃剤として、赤リン系難燃剤20部に替えてリン酸エ
ステル系難燃剤〔製品名:TCP、大八化学工業所
(株)製〕23部を用いるほかは実施例1と同様にして
ポリウレタンを凝固させ、脱溶媒、乾燥させてポリウレ
タン多孔質膜を有するシート状物を得た。該シート状物
は、厚さ0.8mmで、湿式凝固時においては表面は平
滑であったが、乾燥後においては脱溶媒不足のようなヘ
タリがあり、表面凹凸が多く、ボリューム感に欠けたも
のであった。Comparative Example 1 As a flame retardant, 20 parts of a red phosphorus flame retardant was used in place of 23 parts of a phosphoric acid ester flame retardant [Product name: TCP, manufactured by Daihachi Chemical Industry Co., Ltd.]. Polyurethane was coagulated in the same manner as in 1, desolventized and dried to obtain a sheet-like material having a polyurethane porous membrane. The sheet-like material had a thickness of 0.8 mm and had a smooth surface during wet coagulation, but after drying, it had a settled surface such as insufficient desolvation, many surface irregularities, and lacked in volume. It was a thing.
【0038】このシート状物の表面に実施例1と同様に
して表皮層を設け、皮革様シート状物を製造した。この
皮革様シート状物は、耐加水分解性は良好であったが、
耐光性に劣り、FMVSS−302規格による難燃性
(燃焼速度)は93mm/分であった。A skin layer was provided on the surface of this sheet material in the same manner as in Example 1 to produce a leather-like sheet material. Although this leather-like sheet had good hydrolysis resistance,
The light resistance was poor, and the flame retardancy (combustion rate) according to the FMVSS-302 standard was 93 mm / min.
【0039】[0039]
【発明の効果】本発明によれば、湿式凝固性、外観、風
合いを損なうことなく、難燃性に優れた皮革様シート状
物を得ることができる。EFFECTS OF THE INVENTION According to the present invention, a leather-like sheet material having excellent flame retardancy can be obtained without impairing the wet coagulation property, appearance and texture.
【図1】本発明により得られる皮革様シート状物の層構
成の一例を示す断面模式図である。FIG. 1 is a schematic sectional view showing an example of the layer structure of a leather-like sheet material obtained by the present invention.
【図2】本発明により得られる皮革様シート状物の層構
成の一例を示す断面模式図である。FIG. 2 is a schematic cross-sectional view showing an example of the layer structure of a leather-like sheet material obtained by the present invention.
【図3】本発明により得られる皮革様シート状物の層構
成の一例を示す断面模式図である。FIG. 3 is a schematic cross-sectional view showing an example of the layer structure of a leather-like sheet material obtained by the present invention.
10 繊維基材層 21 繊維基材に含浸凝固されて形成されたポリウレタ
ン多孔膜層 22 塗布後凝固されて形成されたポリウレタン多孔膜
層 30 接着層 40 表皮層10 Fiber Substrate Layer 21 Polyurethane Porous Membrane Layer Formed by Impregnation into Fiber Substrate 22 Polyurethane Porous Membrane Layer Formed by Coagulation After Application 30 Adhesive Layer 40 Skin Layer
───────────────────────────────────────────────────── フロントページの続き (51)Int.Cl.5 識別記号 庁内整理番号 FI 技術表示箇所 B32B 27/40 7016−4F C08K 3/32 C08L 75/04 NFY 8620−4J D06N 3/18 7141−4F ─────────────────────────────────────────────────── ─── Continuation of the front page (51) Int.Cl. 5 Identification code Internal reference number FI Technical display location B32B 27/40 7016-4F C08K 3/32 C08L 75/04 NFY 8620-4J D06N 3/18 7141- 4F
Claims (3)
重量部に対して赤リン系難燃剤5〜40重量部を含有す
るポリカーボネート系ポリウレタンの溶剤溶液を繊維基
材に含浸、および/または塗布したのち、該ポリウレタ
ンの非溶剤で凝固させて繊維基材上にポリウレタンの多
孔質膜を形成させ、次いで該多孔質膜表面に表皮層を設
けることを特徴とする皮革様シート状物の製造方法。1. A polycarbonate-based polyurethane 100
A fiber base material is obtained by impregnating and / or applying a solvent solution of a polycarbonate-based polyurethane containing 5 to 40 parts by weight of a red phosphorus flame retardant with respect to parts by weight, and then coagulating with a non-solvent of the polyurethane. A method for producing a leather-like sheet, comprising forming a polyurethane porous film on the surface and then providing a skin layer on the surface of the porous film.
して赤リン系難燃剤を5〜40重量部含有する接着層を
介して設けられている請求項1記載の皮革様シート状物
の製造方法。2. The method for producing a leather-like sheet material according to claim 1, wherein the skin layer is provided via an adhesive layer containing 5 to 40 parts by weight of a red phosphorus flame retardant with respect to 100 parts by weight of polyurethane. ..
有するポリウレタンからなる請求項1または2記載の皮
革様シート状物の製造方法。3. The method for producing a leather-like sheet material according to claim 1, wherein the adhesive layer and / or the skin layer is made of durable polyurethane.