JPH0379689A - Method for coating hand-rail belt - Google Patents

Method for coating hand-rail belt

Info

Publication number
JPH0379689A
JPH0379689A JP21938789A JP21938789A JPH0379689A JP H0379689 A JPH0379689 A JP H0379689A JP 21938789 A JP21938789 A JP 21938789A JP 21938789 A JP21938789 A JP 21938789A JP H0379689 A JPH0379689 A JP H0379689A
Authority
JP
Japan
Prior art keywords
abrasive
belt
polished
coating
detergent
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP21938789A
Other languages
Japanese (ja)
Other versions
JPH089477B2 (en
Inventor
Masashi Tsukamoto
塚本 政司
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
NIPPON REJIBON KK
Nippon Resibon Corp
Original Assignee
NIPPON REJIBON KK
Nippon Resibon Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by NIPPON REJIBON KK, Nippon Resibon Corp filed Critical NIPPON REJIBON KK
Priority to JP21938789A priority Critical patent/JPH089477B2/en
Publication of JPH0379689A publication Critical patent/JPH0379689A/en
Publication of JPH089477B2 publication Critical patent/JPH089477B2/en
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Abstract

PURPOSE:To coat a hand-rail belt with a coating film having sufficient gloss and resistant to abrasion, peeling and cracking in a short time in high efficiency by applying a detergent to a hand-rail belt, polishing with abrasives having three grain sizes and coating the polished surface with a specific coating agent. CONSTITUTION:The surface of a hand-rail belt is coated with preferably an oily detergent and left standing for a prescribed period to effect the flotation of the stain. The treated surface is polished in wet state with an abrasive having a grain size of about #400. The polished surface is further polished with an abrasive having a grain size of #150-400 and then with an abrasive of #500-600. The surface is finally coated with a coating agent composed mainly of an acrylic copolymer resin.

Description

【発明の詳細な説明】 〈産業上の利用分野〉 この発明は手すりベルトのコーティング方法に関する。[Detailed description of the invention] <Industrial application field> The present invention relates to a method of coating a handrail belt.

〈従来の技術〉 エスカレータやオートラン等において、移動式の手すり
ベルトが用いられている。
<Prior Art> Movable handrail belts are used on escalators, autoruns, etc.

この手すりベルトは、多数の人の手垢や汚れ。This handrail belt is covered with dirt and grime from many people's hands.

或は駆動装置との接触による摩耗や油汚れにより、その
表面が黒く汚れてくる。
Alternatively, the surface becomes black and dirty due to wear and oil stains caused by contact with the drive device.

このような汚れを研磨により削り取り、その後ベルト表
面に合成樹脂皮膜をコーティングする手すりベルトのコ
ーティング方法が従来より知られている。
A handrail belt coating method has been known in which such dirt is removed by polishing, and then the belt surface is coated with a synthetic resin film.

〈発明が解決しようとする問題点〉 しかし、従来の方法では通常の研磨材による研磨を行っ
ていたため、油汚れ等により研磨材の砥粒が目詰まりし
、研削するのに長時間を要する欠点があった。また、研
磨した粉塵が空中に浮遊し、数時間後に降下するため附
近に粉塵が舞い降りてウィンド、ショーケース、商品等
をよごし清掃が非常に面倒である等の問題があった。
<Problems to be solved by the invention> However, in the conventional method, polishing was performed using a normal abrasive material, which had the disadvantage that the abrasive grains of the abrasive material were clogged with oil stains, etc., and it took a long time to complete the grinding process. was there. In addition, since the polished dust floats in the air and descends after several hours, the dust falls in the vicinity, soiling windows, showcases, products, etc., and making cleaning very troublesome.

更に、合成樹脂のコーティングに乾燥時間も含めて12
〜15時間も要する欠点があった。
Furthermore, including drying time for synthetic resin coating, 12
There was a drawback that it required ~15 hours.

〈発明の概要〉 本発明は上記した従来の方法の欠点を解決するためにな
されたもので、短時間で粉塵の発生もなく、シかも強固
なコーテイング面を得られるコーティング方法を提供す
ることを目的とするものである。
<Summary of the Invention> The present invention has been made to solve the drawbacks of the conventional methods described above, and aims to provide a coating method that can obtain a strong coating surface in a short time without generating dust. This is the purpose.

本発明においては、まず手すりベルトの表面に洗剤を塗
布して所定時間放置する。塗布する洗剤としては油性洗
剤が好ましく、また塗布後好ましくは2分から3分の間
装置して洗剤成分が汚れの内部に浸透するのを待つ。所
定時間経過したら略粒度#400の研磨材により手すり
ベルトの表面を研磨する。この研磨は洗剤により濡れた
ベルト表面を研磨する湿式研磨である。研磨材としては
、不織布に研磨粒子を接着したナイロンバット等を用い
るのが望ましい、この場合研磨粒子は研磨面の粗さが粒
度#400に相当する粒子とする。
In the present invention, detergent is first applied to the surface of the handrail belt and left for a predetermined period of time. The detergent to be applied is preferably an oil-based detergent, and after application, it is preferably left in the apparatus for 2 to 3 minutes to wait for the detergent components to penetrate into the dirt. After a predetermined period of time has elapsed, the surface of the handrail belt is polished with an abrasive having a particle size of approximately #400. This polishing is wet polishing in which the surface of the belt is polished using a detergent. As the abrasive material, it is desirable to use a nylon bat or the like in which abrasive particles are adhered to a nonwoven fabric. In this case, the abrasive particles are particles whose polished surface roughness corresponds to particle size #400.

ここで、略粒度#400の研磨材と限定したのはこれ以
下では汚れを除去するのに時間がかかりすぎ、またこれ
以上粗い粒子であると固着した汚れの表面を引っかいて
滑るだけで汚れ除去の効果かないためである。
Here, we limited the abrasive material to a particle size of approximately #400 because if it is less than this, it will take too long to remove the dirt, and if the particles are coarser than this, the dirt will be removed by simply scratching and sliding on the surface of the stuck dirt. This is because it has no effect.

以上のように洗剤により汚れを浮き上がらせておいて、
適当な粒子の研磨材により研磨することにより、短時間
に効率的に汚れを落とすことが出来る。しかも、この研
磨は湿式であるため粉塵が生ずることがない。
As mentioned above, use detergent to lift the dirt,
By polishing with an appropriate abrasive particle, dirt can be removed efficiently in a short time. Furthermore, since this polishing is a wet process, no dust is generated.

上記により汚れを除去したら、次いで粒度#150〜#
400の研磨材により手すりベルトの表面を研磨する。
After removing the dirt as described above, the particle size is #150 to #
The surface of the handrail belt is polished with a 400% abrasive.

これによりベルト表面の傷や劣化した部分を削り取り、
同時にベルト表面に2〜3μmの山谷を形成する。ここ
で、粒度#150〜#400と限定したのは、前工程で
表面の汚れが除去されているためそれほどの研磨は必要
なく、またこれ以上の粒度で研磨すると、研磨面の山が
高くなりすぎるためである。山が高くなり過ぎると次工
程で合成樹脂のコーティングを数回行って厚塗りにしな
ければならず1重ね塗りして膜厚を厚くすると結合力が
弱くなり剥離の原因となるためである。なお、粒度#1
50〜3400以下の研磨であると十分な山谷が形成で
きない。
This removes scratches and deteriorated parts of the belt surface,
At the same time, peaks and valleys of 2 to 3 μm are formed on the belt surface. Here, we limited the grain size to #150 to #400 because dirt on the surface has been removed in the previous process, so there is no need for much polishing, and if we polish with a grain size larger than this, the peaks on the polished surface will become high. This is because it is too much. This is because if the peaks become too high, the synthetic resin coating must be applied several times in the next step to make it thicker, and if one layer is applied to increase the film thickness, the bonding force will weaken and cause peeling. In addition, particle size #1
If the polishing is less than 50 to 3400, sufficient peaks and valleys cannot be formed.

次ぎに更に粒度#500〜8600の研磨材により手す
りベルトの表面を研磨し1粒度#150〜#400の研
磨材による研磨傷を消すと同時に2〜3μmの山谷の斜
面に更に0.3〜0.5μの細かな山谷を形成する。こ
の2〜3μと0.3〜0.5μの複合的な山谷により、
次工程で塗布される合成樹脂皮膜を強固に結合できる。
Next, the surface of the handrail belt is further polished with an abrasive with a grain size of #500 to #8600, and at the same time, the scratches caused by the abrasive with a grain size of #150 to #400 are removed, and at the same time, the slopes of the peaks and valleys of 2 to 3 μm are further polished with 0.3 to 0.0 μm. Forms fine peaks and valleys of .5μ. Due to the composite peaks and valleys of 2 to 3μ and 0.3 to 0.5μ,
It can firmly bond the synthetic resin film applied in the next process.

また、同時に光を乱反射してベルト表面に十分な光沢を
与えることが出来る。
Moreover, at the same time, it is possible to diffusely reflect light and give sufficient gloss to the belt surface.

上記工程によりベルト表面の研磨を終了したら、この状
態でアクリル共重合樹脂を主成分としたコーティング剤
を塗布する。このコーティング剤は3回程度塗布して0
.015mm〜0.02mrnの被膜を形成するのが好
ましい、アクリル共重合樹脂を主成分としたコーティン
グ剤は水溶性塗布剤であるため塗布が簡単であり、且つ
乾燥時間が10分〜20分と短く、3回コーティングし
てもエスカレータ−機をコグティジグ施工するのに2時
間程度しか必要としない。
After polishing the belt surface through the above steps, a coating agent containing acrylic copolymer resin as a main component is applied in this state. Apply this coating agent about 3 times and
.. It is preferable to form a film of 0.015 mm to 0.02 mrn. The coating agent mainly composed of acrylic copolymer resin is easy to apply because it is a water-soluble coating agent, and the drying time is short at 10 to 20 minutes. Even after coating three times, it only takes about two hours to install the escalator using a cogti jig.

〈実施例〉 次ぎに実施例を示す。<Example> Next, examples will be shown.

第1図はエスカレータ用の手すりベルトの断面図であり
、この手すりベルトは厚織帆布芯体1、化粧ゴム層2か
ら構成されている。(ア)は化粧ゴム層2の表面に汚れ
及び老化部3が形成されている状態を示している。
FIG. 1 is a sectional view of a handrail belt for an escalator, and this handrail belt is composed of a thick woven canvas core 1 and a decorative rubber layer 2. (A) shows a state in which dirt and aged parts 3 are formed on the surface of the decorative rubber layer 2.

エスカレータ−を停止状態とし先ず上部に露呈している
左右のベルトに下記成分の油性洗剤を5倍〜20倍に稀
釈した液をベルト表面に塗布し。
With the escalator in a stopped state, first, on the left and right belts exposed at the top, a solution prepared by diluting an oil-based detergent with the following ingredients 5 to 20 times is applied to the belt surface.

2分〜3分放置して、洗剤が汚れの内部へ浸透するまで
待つ、不織布に研磨粒子を装着したスコッチブライトS
/Fのハンドバット(粒度#400に相当)に該洗剤を
含浸させて汚れた面を削除する。露呈したベルト片面の
汚れを削除した後ベルトを反転して残りの片面を同じ工
程にて汚れを削除する(イ)。その際エスカレータ−の
周囲特に内側板を洗剤にて汚さぬ様に事前にマスキング
する。
Leave it for 2 to 3 minutes and wait until the detergent penetrates into the dirt. Scotch Brite S is a non-woven fabric with abrasive particles attached.
/F hand vat (corresponding to particle size #400) is impregnated with the detergent and the soiled surface is removed. After removing the dirt on one side of the exposed belt, turn the belt over and remove the dirt on the remaining side in the same process (a). At that time, mask the area around the escalator, especially the inner panel, in advance so as not to stain it with detergent.

(洗剤成分) 非イオン系界面活性剤   グリコール系溶剤陰イオン
系界面活性剤   腐食防止剤ケイ酸塩系ビルダー  
  水 キレート剤 ベルト表面の汚れを削除した後、ベルト表面の「キズ」
及び老化した部分をオービタルサンダ又はベルトサンダ
に粒度#150〜#400のサンドペーパーを取付けて
研削し、「キズ」及び老化部分を除去し2μ〜3μの山
谷を形成する。さらに粒度#500〜#600のサンド
ベーパーを取付けて研磨し1粒度#240〜#320の
研磨による研削傷を消すと共に、2μ〜3μの山谷の斜
面に0.3μ〜0.5μの複合山谷4を形成する(つ)
(Detergent ingredients) Nonionic surfactant Glycol solvent Anionic surfactant Corrosion inhibitor Silicate builder
After removing dirt on the belt surface with water chelating agent, "scratches" on the belt surface
The aged part is ground using an orbital sander or a belt sander with sandpaper having a grain size of #150 to #400 attached to remove "scratches" and aged parts, and form peaks and valleys of 2 to 3 microns. Furthermore, a sand vapor with a grain size of #500 to #600 is installed and polished to erase the scratches caused by polishing with a grain size of #240 to #320, and a composite peak and valley 4 of 0.3 μ to 0.5 μ is added to the slope of a mountain and valley of 2 μ to 3 μ. form (tsu)
.

ベルト表面に付着した研削屑を清掃した後、アクリルウ
レタン共重合樹脂を主成分とした下記コーティング剤を
布タンパに含ませて薄く塗布する。
After cleaning the grinding debris adhering to the belt surface, a cloth tamper is soaked with the following coating agent, which is mainly composed of acrylic urethane copolymer resin, and applied thinly.

1回塗布後10分〜15分乾燥させ、3回塗布する。3
回目を塗布後の乾燥時間は30分〜40分と長く乾燥さ
せ塗布面の完全硬化を待つ3表面完全硬化後ベルトを反
転し、残り片面を同じ工程にてコーティングし、被覆5
を形成する(1)。
After applying once, dry for 10 to 15 minutes and apply three times. 3
The drying time after the second application is 30 to 40 minutes, allowing the coated surface to completely harden. 3. After the surface is completely hardened, turn the belt over and coat the remaining side in the same process.
(1).

(コーティング剤成分) アクリル−ウレタン共重合樹脂 高融点ワックスエマルション レベリング剤 界面活性剤 可塑剤 防腐剤 水 (コーチイ 不揮発分: P H(25℃): 粘度(25℃): 比重(25℃): ング剤物性値) 21.0±2.0% 8.8±0.5 11.0±5.Oc、p、s 1.033士0.004 以上の工程において、 研磨作業は洗剤によりき わめて簡単に汚れを落とすことが出来るため、労力が従
来の173で済み、作業時間も1時間と従来の173に
削減できた。また湿式研磨であるため研磨作業中の粉塵
も皆無に等しかった。更に、コーティング作業はアクリ
ルウレタン共重合体を主成分としたものを用いているた
め、自動車のワックス掛けのように簡単であり、乾燥は
10〜20分ですみ、3回コーティングでエスカレータ
−機あたり2時間程度しか要しなかった。
(Coating agent components) Acrylic-urethane copolymer resin High melting point wax Emulsion leveling agent Surfactant Plasticizer Preservative Water (Kochii non-volatile content: PH (25℃): Viscosity (25℃): Specific gravity (25℃): Ng Drug physical property value) 21.0±2.0% 8.8±0.5 11.0±5. Oc, p, s 1.033 and 0.004 In the above process, the polishing work can remove dirt very easily with detergent, so the labor required is only 173 lbs., and the working time is 1 hour, which is less than the conventional 173 lbs. was able to be reduced to Also, since it was a wet polishing process, there was almost no dust during the polishing process. Furthermore, since the coating process uses a material mainly composed of acrylic urethane copolymer, it is as easy as waxing a car, takes only 10 to 20 minutes to dry, and can be coated three times per escalator machine. It only took about 2 hours.

得られた被1!15は0.O15〜0.02mmの厚さ
であり、この被覆5表面に第2図に示すように、先端に
Rを設けた棒材を6kgの荷重を掛けて押し当て、17
0サイクル/分で50.000回の摩擦を与えた。その
結果、すり切れを全く生じなかった。
The obtained number 1!15 is 0. As shown in FIG. 2, a bar with a radius at the tip is pressed against the surface of this coating 5 with a load of 6 kg, and the thickness is 15 to 0.02 mm.
50,000 rubs were applied at 0 cycles/min. As a result, no wear occurred.

更に第3図に示すように、被$1[5を下側にして80
サイクル/分で3.000回、90’屈曲させた。その
結果剥離や割れ等を全く生じなかった。
Furthermore, as shown in Figure 3, the amount of $1 [5 is on the bottom and
90' bends were made 3.000 cycles/min. As a result, no peeling or cracking occurred.

〈発明の効果〉 以上説明したように、本発明の手すりベルトのコーティ
ング方法は、手すりベルトの表面に洗剤を塗布して所定
時間放置した後、略粒度#400の研磨材により手すり
ベルトの表面を湿式研磨し、次いで粒度#240〜#3
20の研磨材により手すりベルトの表面を研磨し、更に
粒度#500〜#600の研磨材により手すりベルトの
表面を研磨し、この状態でアクリル共重合樹脂を主成分
としたコーティング剤を塗布するため5作業性が良い上
1作業時間が短くて済み、しかも結合度が高く容易にす
り切れや剥離或は割れを生ずることがなく、更に十分な
光沢を有するコーティングを得ることが可能である。
<Effects of the Invention> As explained above, in the method of coating a handrail belt of the present invention, after applying detergent to the surface of the handrail belt and leaving it for a predetermined period of time, the surface of the handrail belt is coated with an abrasive material having a particle size of approximately #400. Wet polishing, then grain size #240~#3
In order to polish the surface of the handrail belt with an abrasive of #20 and further polish the surface of the handrail belt with an abrasive of #500 to #600 in particle size, and in this state apply a coating agent mainly composed of acrylic copolymer resin. 5. It has good workability and requires only a short working time, has a high degree of bonding and does not easily wear off, peel or crack, and can provide a coating with sufficient gloss.

【図面の簡単な説明】[Brief explanation of drawings]

第1図は本発明方法の一実施例の説明図、第2図と第3
図は試験方法の説明図である。 1:厚縁帆布芯体、2:化粧ゴム層、3:汚れ及び老化
部、4:複合山谷、5:被覆。
Figure 1 is an explanatory diagram of one embodiment of the method of the present invention, Figures 2 and 3
The figure is an explanatory diagram of the test method. 1: Thick-edged canvas core, 2: Decorative rubber layer, 3: Dirt and aging area, 4: Composite peaks and valleys, 5: Covering.

Claims (1)

【特許請求の範囲】 手すりベルトの表面に洗剤を塗布して所定時間放置した
後、略粒度#400の研磨材により手すりベルトの表面
を湿式研磨し、 次いで粒度#150〜#400の研磨材により手すりベ
ルトの表面を研磨し、 更に粒度#500〜#600の研磨材により手すりベル
トの表面を研磨し、 この状態でアクリル共重合樹脂を主成分としたコーティ
ング剤を塗布する、 ことを特徴とする手すりベルトのコーティング方法。
[Claims] After applying a detergent to the surface of the handrail belt and leaving it for a predetermined period of time, the surface of the handrail belt is wet-polished with an abrasive material with a particle size of approximately #400, and then with an abrasive material with a particle size of #150 to #400. It is characterized by polishing the surface of the handrail belt, further polishing the surface of the handrail belt with an abrasive with a particle size of #500 to #600, and applying a coating agent mainly composed of acrylic copolymer resin in this state. How to coat handrail belts.
JP21938789A 1989-05-17 1989-08-25 Handrail belt coating method Expired - Lifetime JPH089477B2 (en)