JP7194789B2 - Articles and methods of manufacturing articles - Google Patents

Articles and methods of manufacturing articles Download PDF

Info

Publication number
JP7194789B2
JP7194789B2 JP2021126669A JP2021126669A JP7194789B2 JP 7194789 B2 JP7194789 B2 JP 7194789B2 JP 2021126669 A JP2021126669 A JP 2021126669A JP 2021126669 A JP2021126669 A JP 2021126669A JP 7194789 B2 JP7194789 B2 JP 7194789B2
Authority
JP
Japan
Prior art keywords
polyamide resin
molded article
semi
aromatic polyamide
article according
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
JP2021126669A
Other languages
Japanese (ja)
Other versions
JP2021181579A (en
Inventor
章人 岡元
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Mitsubishi Engineering Plastics Corp
Original Assignee
Mitsubishi Engineering Plastics Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Mitsubishi Engineering Plastics Corp filed Critical Mitsubishi Engineering Plastics Corp
Priority to JP2021126669A priority Critical patent/JP7194789B2/en
Publication of JP2021181579A publication Critical patent/JP2021181579A/en
Priority to JP2022198053A priority patent/JP7310089B2/en
Priority to JP2022198052A priority patent/JP7310088B2/en
Application granted granted Critical
Publication of JP7194789B2 publication Critical patent/JP7194789B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Description

本発明は、成形品および成形品の製造方法に関する。特に自動車に搭載するカメラ部品に適した成形品および成形品の製造方法に関する。 The present invention relates to molded articles and methods of manufacturing molded articles. In particular, the present invention relates to a molded article suitable for camera parts mounted on automobiles and a method for manufacturing the molded article.

代表的なエンジニアリングプラスチックであるポリアミド樹脂は、加工が容易であり、さらに、機械的物性、電気特性、耐熱性、その他の物理的および化学的特性に優れている。このため、車両部品、電気電子機器部品、その他の精密機器部品等に幅広く使用されている。
例えば、特許文献1には、テレフタル酸単位を60~100モル%含有するジカルボン酸単位と1,9-ジアミノノナン単位および/または2-メチル-1,8-ジアミノオクタン単位を60~100モル%含有するジアミン単位とを有するポリアミド(A)および繊維状強化材(B)を溶融混練してなり、ポリアミド(A)の含有率が50~80質量%であり繊維状強化材(B)の含有率が20~50質量%であるポリアミド組成物を成形してなるカメラモジュールのバレルまたはホルダであって、上記繊維状強化材(B)の溶融混練前における平均長さが300μm以下であるカメラモジュールのバレルまたはホルダが開示されている。
Polyamide resins, which are representative engineering plastics, are easy to process and have excellent mechanical properties, electrical properties, heat resistance, and other physical and chemical properties. Therefore, it is widely used for vehicle parts, electrical and electronic equipment parts, and other precision equipment parts.
For example, in Patent Document 1, dicarboxylic acid units containing 60 to 100 mol% of terephthalic acid units and 1,9-diaminononane units and/or 60 to 100 mol% of 2-methyl-1,8-diaminooctane units are disclosed. A polyamide (A) having a diamine unit and a fibrous reinforcing material (B) are melt-kneaded, and the content of the polyamide (A) is 50 to 80% by mass and the content of the fibrous reinforcing material (B) A camera module barrel or holder formed by molding a polyamide composition having a content of 20 to 50% by mass, wherein the fibrous reinforcing material (B) has an average length of 300 μm or less before melt-kneading. A barrel or holder is disclosed.

特開2010-286544号公報JP 2010-286544 A

上記特許文献1について本発明者が検討したところ、上記特許文献1では、繊維状充填材を配合しているが、機械的強度が不十分であることが分かった。また、カメラ部品などの精密機械部品では、水分が透過しにくいことも求められる。本発明は、かかる課題を解決することを目的としたものであって、機械的強度に優れ、かつ、水分が透過しにくい成形品を提供することを目的とする。 When the present inventor examined Patent Document 1, it was found that the mechanical strength was insufficient in Patent Document 1, although a fibrous filler was blended. In addition, precision machine parts such as camera parts are required to be less permeable to moisture. An object of the present invention is to solve such problems, and an object thereof is to provide a molded article which is excellent in mechanical strength and impermeable to moisture.

上記課題のもと、本発明者が検討を行った結果、末端カルボキシル基濃度が末端アミノ基濃度よりも高い半芳香族ポリアミド樹脂を用い、かつ、数平均繊維長が300μmを超える繊維から成形される成形品とすることにより、半芳香族ポリアミド樹脂と繊維の密着性を向上させ、機械的強度を向上させ、かつ、水分を透過しにくくしうることを見出し、本発明を完成するに至った。
具体的には、下記手段<1>により、好ましくは<2>~<15>により、上記課題は解決された。
<1>半芳香族ポリアミド樹脂と、数平均繊維長が300μmを超える繊維を含み、前記半芳香族ポリアミド樹脂の末端カルボキシル基濃度が末端アミノ基濃度よりも高い、ポリアミド樹脂組成物から成形された成形品。
<2>前記繊維が炭素繊維およびガラス繊維から選択される少なくとも1種である、<1>に記載の成形品。
<3>前記繊維が、表面処理剤および集束剤の少なくとも一方で処理されている、<1>または<2>に記載の成形品。
<4>前記繊維の数平均繊維長が1.0mm~6.0mmである、<1>~<3>のいずれか1つに記載の成形品。
<5>前記末端カルボキシル基濃度と末端アミノ基濃度の差が40~100μ当量/gである、<1>~<4>のいずれか1つに記載の成形品。
<6>前記半芳香族ポリアミド樹脂が、ジアミン由来の構成単位とジカルボン酸由来の構成単位から構成され、ジアミン由来の構成単位の70モル%以上がキシリレンジアミンに由来し、ジカルボン酸由来の構成単位の70モル%以上が炭素数4~20のα,ω-直鎖脂肪族ジカルボン酸に由来する、<1>~<5>のいずれか1つに記載の成形品。
<7>前記半芳香族ポリアミド樹脂が、ジアミン由来の構成単位とジカルボン酸由来の構成単位から構成され、ジアミン由来の構成単位の70モル%以上がキシリレンジアミンに由来し、ジカルボン酸由来の構成単位の70モル%以上がアジピン酸に由来する、<1>~<5>のいずれか1つに記載の成形品。
<8>さらに、黒色着色剤を含む、<1>~<7>のいずれか1つに記載の成形品。
<9>さらに、タルクを含む、<1>~<8>のいずれか1つに記載の成形品。
<10>さらに、黒色着色剤とタルクを含み、前記成形品における、黒色着色剤とタルクの質量比(黒色着色剤/タルク)が1.5~2.5である、<1>~<7>のいずれか1つに記載の成形品。
<11>射出成形品である、<1>~<10>のいずれか1つに記載の成形品。
<12>カメラ部品である、<1>~<11>のいずれか1つに記載の成形品。
<13>前記カメラ部品の最大長さが、15~40mmである、<12>に記載の成形品。
<14>前記カメラ部品が、前記ポリアミド樹脂組成物に由来する部材を含み、前記部材の割合が、1~99質量%である、<12>または<13>に記載の成形品。
<15>半芳香族ポリアミド樹脂と、数平均繊維長が300μmを超える繊維を含み、前記半芳香族ポリアミド樹脂の末端カルボキシル基濃度が末端アミノ基濃度よりも高い、ポリアミド樹脂組成物を射出成形することを含む、<1>~<14>のいずれか1つに記載の成形品の製造方法。
Based on the above problems, the present inventors conducted studies and found that a semi-aromatic polyamide resin having a terminal carboxyl group concentration higher than a terminal amino group concentration was used, and a fiber having a number average fiber length exceeding 300 µm was molded. The inventors have found that by forming a molded product that is made of a semi-aromatic polyamide resin and the fiber, the adhesion between the semi-aromatic polyamide resin and the fiber can be improved, the mechanical strength can be improved, and moisture can be made difficult to permeate, and the present invention has been completed. .
Specifically, the above problems have been solved by the following means <1>, preferably by <2> to <15>.
<1> Molded from a polyamide resin composition containing a semi-aromatic polyamide resin and fibers having a number average fiber length of more than 300 μm, wherein the terminal carboxyl group concentration of the semi-aromatic polyamide resin is higher than the terminal amino group concentration Molding.
<2> The molded article according to <1>, wherein the fiber is at least one selected from carbon fiber and glass fiber.
<3> The molded article according to <1> or <2>, wherein the fibers are treated with at least one of a surface treatment agent and a sizing agent.
<4> The molded article according to any one of <1> to <3>, wherein the number average fiber length of the fibers is 1.0 mm to 6.0 mm.
<5> The molded article according to any one of <1> to <4>, wherein the difference between the terminal carboxyl group concentration and the terminal amino group concentration is 40 to 100 μeq/g.
<6> The semi-aromatic polyamide resin is composed of diamine-derived structural units and dicarboxylic acid-derived structural units, and 70 mol% or more of the diamine-derived structural units are derived from xylylenediamine, and the dicarboxylic acid-derived structure The molded article according to any one of <1> to <5>, wherein 70 mol% or more of the units are derived from the α,ω-linear aliphatic dicarboxylic acid having 4 to 20 carbon atoms.
<7> The semi-aromatic polyamide resin is composed of diamine-derived structural units and dicarboxylic acid-derived structural units, and 70 mol% or more of the diamine-derived structural units are derived from xylylenediamine, and the dicarboxylic acid-derived structure The molded article according to any one of <1> to <5>, wherein 70 mol% or more of the units are derived from adipic acid.
<8> The molded article according to any one of <1> to <7>, further comprising a black colorant.
<9> The molded article according to any one of <1> to <8>, further comprising talc.
<10> Further, <1> to <7, wherein a black coloring agent and talc are included, and the mass ratio of the black coloring agent to talc (black coloring agent/talc) in the molded article is 1.5 to 2.5. The molded article according to any one of >.
<11> The molded article according to any one of <1> to <10>, which is an injection molded article.
<12> The molded article according to any one of <1> to <11>, which is a camera part.
<13> The molded article according to <12>, wherein the camera component has a maximum length of 15 to 40 mm.
<14> The molded article according to <12> or <13>, wherein the camera component contains a member derived from the polyamide resin composition, and the proportion of the member is 1 to 99% by mass.
<15> Injection molding a polyamide resin composition containing a semi-aromatic polyamide resin and fibers having a number average fiber length of more than 300 μm, wherein the terminal carboxyl group concentration of the semi-aromatic polyamide resin is higher than the terminal amino group concentration. The method for producing a molded article according to any one of <1> to <14>, comprising:

本発明により、機械的強度に優れ、水分が透過しにくい成形品を提供可能になった。 The present invention has made it possible to provide molded articles that are excellent in mechanical strength and impermeable to moisture.

水分透過係数の測定装置を示す概略図である。1 is a schematic diagram showing a device for measuring water permeability coefficient; FIG.

以下において、本発明の内容について詳細に説明する。尚、本明細書において「~」とはその前後に記載される数値を下限値および上限値として含む意味で使用される。 The contents of the present invention will be described in detail below. In this specification, the term "~" is used to mean that the numerical values before and after it are included as the lower limit and the upper limit.

本発明の成形品は、半芳香族ポリアミド樹脂と、数平均繊維長が300μmを超える繊維を含み、前記半芳香族ポリアミド樹脂の末端カルボキシル基濃度が末端アミノ基濃度よりも高い、ポリアミド樹脂組成物から成形された成形品であることを特徴とする。
末端カルボキシル基濃度が末端アミノ基濃度よりも高い半芳香族ポリアミド樹脂を用い、かつ、数平均繊維長が300μmを超える繊維を用いることにより、半芳香族ポリアミド樹脂の繊維に対する密着性が向上し、機械的強度が高い成形品が得られる。さらに、水分が透過しにくい成形品が得られる。
The molded article of the present invention comprises a semi-aromatic polyamide resin and fibers having a number average fiber length of more than 300 μm, and the terminal carboxyl group concentration of the semi-aromatic polyamide resin is higher than the terminal amino group concentration, a polyamide resin composition. It is characterized by being a molded article molded from.
By using a semi-aromatic polyamide resin having a terminal carboxyl group concentration higher than a terminal amino group concentration and using a fiber having a number average fiber length exceeding 300 μm, the adhesion of the semi-aromatic polyamide resin to the fiber is improved, Molded products with high mechanical strength can be obtained. Furthermore, a molded article that is difficult to permeate with moisture can be obtained.

<半芳香族ポリアミド樹脂>
本発明の成形品は、半芳香族ポリアミド樹脂を含む。
ここで、半芳香族ポリアミド樹脂とは、ジアミン由来の構成単位とジカルボン酸由来の構成単位から構成され、ジアミン由来の構成単位およびジカルボン酸由来の構成単位の合計構成単位の30~70モル%が芳香環を含む構成単位であることをいい、ジアミン由来の構成単位およびジカルボン酸由来の構成単位の合計構成単位の40~60モル%が芳香環を含む構成単位であることが好ましい。
<Semi-aromatic polyamide resin>
The molded article of the present invention contains a semi-aromatic polyamide resin.
Here, the semi-aromatic polyamide resin is composed of diamine-derived structural units and dicarboxylic acid-derived structural units, and 30 to 70 mol% of the total structural units of the diamine-derived structural units and dicarboxylic acid-derived structural units It refers to a structural unit containing an aromatic ring, and preferably 40 to 60 mol % of the total structural units of the diamine-derived structural unit and the dicarboxylic acid-derived structural unit are structural units containing an aromatic ring.

本発明で用いる半芳香族ポリアミド樹脂は、末端カルボキシル基濃度が末端アミノ基濃度よりも高い。このような構成とすることにより、繊維と半芳香族ポリアミド樹脂の密着性を向上させることができる。
本発明における末端カルボキシル基濃度と末端アミノ基濃度の差は40~100μ当量/gであることが好ましい。このような範囲とすることにより、繊維との密着性をより向上させることができる。
前記末端カルボキシル基濃度と末端アミノ基濃度の差は、下限値が、45μ当量/g以上であることが好ましく、47μ当量/g以上であることがより好ましい。前記末端カルボキシル基濃度と末端アミノ基濃度の差は、上限値が、90μ当量/g以下であることが好ましく、80μ当量/g以下であることがより好ましく、70μ当量/g以下であることがさらに好ましく、65μ当量/g以下であることが一層好ましく、55μ当量/g以下であることがより一層好ましい。
また、本発明で用いる半芳香族ポリアミド樹脂は、末端アミノ基濃度([NH2])が好ましくは100μ当量/g未満、より好ましくは5~75μ当量/g、さらに好ましくは10~60μ当量/g、一層好ましくは20~50μ当量/gである。また、本発明で用いる半芳香族ポリアミド樹脂は、末端カルボキシル基濃度([COOH])が、好ましくは150μ当量/g未満、より好ましくは20~120μ当量/g、さらに好ましくは40~110μ当量/g、一層好ましくは50~100μ当量/g、より一層好ましくは75~100μ当量/gである。
さらに、末端カルボキシル基濃度に対する末端アミノ基濃度の比([NH2]/[COOH])は、0.7以下が好ましく、0.6以下がより好ましく、0.5以下がさらに好ましい。前記比が0.7よりも大きいものは、半芳香族ポリアミド樹脂を重合する際に、分子量の制御が難しくなる場合がある。前記末端カルボキシル基濃度に対する末端アミノ基濃度の比([NH2]/[COOH])の下限値は特に定めるものではないが、例えば、0.2以上であってもよい。
半芳香族ポリアミド樹脂の末端アミノ基濃度および末端カルボキシル基濃度の測定は、後述する実施例に記載の方法に従う。実施例に記載の機器等が廃版等により入手不可能な場合、他の同等の性能を有する機器を用いることができる。以下、他の測定方法についても、同様である。
The semi-aromatic polyamide resin used in the present invention has a terminal carboxyl group concentration higher than a terminal amino group concentration. With such a configuration, the adhesion between the fibers and the semi-aromatic polyamide resin can be improved.
The difference between the terminal carboxyl group concentration and the terminal amino group concentration in the present invention is preferably 40 to 100 μeq/g. By setting it as such a range, the adhesiveness with a fiber can be improved more.
The lower limit of the difference between the terminal carboxyl group concentration and the terminal amino group concentration is preferably 45 μeq/g or more, more preferably 47 μeq/g or more. The upper limit of the difference between the terminal carboxyl group concentration and the terminal amino group concentration is preferably 90 μeq/g or less, more preferably 80 μeq/g or less, and 70 μeq/g or less. More preferably, it is 65 μeq/g or less, and even more preferably 55 μeq/g or less.
In addition, the semi-aromatic polyamide resin used in the present invention preferably has a terminal amino group concentration ([NH 2 ]) of less than 100 μeq/g, more preferably 5 to 75 μeq/g, still more preferably 10 to 60 μeq/g. g, more preferably 20-50 μeq/g. In addition, the semi-aromatic polyamide resin used in the present invention has a terminal carboxyl group concentration ([COOH]) of preferably less than 150 μeq/g, more preferably 20 to 120 μeq/g, still more preferably 40 to 110 μeq/g. g, more preferably 50-100 μeq/g, even more preferably 75-100 μeq/g.
Furthermore, the ratio of terminal amino group concentration to terminal carboxyl group concentration ([NH 2 ]/[COOH]) is preferably 0.7 or less, more preferably 0.6 or less, and even more preferably 0.5 or less. If the ratio is more than 0.7, it may become difficult to control the molecular weight when polymerizing the semi-aromatic polyamide resin. Although the lower limit of the ratio of terminal amino group concentration to terminal carboxyl group concentration ([NH 2 ]/[COOH]) is not particularly defined, it may be, for example, 0.2 or more.
The terminal amino group concentration and the terminal carboxyl group concentration of the semi-aromatic polyamide resin are measured according to the methods described in Examples below. If the devices and the like described in the examples cannot be obtained due to obsolescence or the like, other devices having equivalent performance can be used. The same applies to other measurement methods hereinafter.

本発明で用いる半芳香族ポリアミド樹脂としては、ポリヘキサメチレンテレフタラミド(ポリアミド6T)、ポリヘキサメチレンイソフタラミド(ポリアミド6I)、ポリアミド66/6T、ポリキシリレンアジパミド、ポリキシリレンセバカミド、ポリキシリレンドデカミド、ポリアミド9T、ポリアミド9MT、ポリアミド6I/6T等が挙げられる。
その他、特開2016-138163号公報の段落0020~0058に記載の半芳香族ポリアミド樹脂等も好ましく用いられる。
Semi-aromatic polyamide resins used in the present invention include polyhexamethylene terephthalamide (polyamide 6T), polyhexamethylene isophthalamide (polyamide 6I), polyamide 66/6T, polyxylylene adipamide, polyxylylene bacamide, polyxylylene dedecamide, polyamide 9T, polyamide 9MT, polyamide 6I/6T and the like.
In addition, semi-aromatic polyamide resins and the like described in paragraphs 0020 to 0058 of JP-A-2016-138163 are also preferably used.

上述のような半芳香族ポリアミド樹脂の中でも、成形性、耐熱性の観点から、ジアミン由来の構成単位とジカルボン酸由来の構成単位から構成され、ジアミン由来の構成単位の70モル%以上がキシリレンジアミンに由来し、ジカルボン酸由来の構成単位の70モル%以上が炭素数4~20のα,ω-直鎖脂肪族ジカルボン酸に由来する半芳香族ポリアミド樹脂(以下、「XD系ポリアミド」ということがある)が好ましい。 Among the semi-aromatic polyamide resins as described above, from the viewpoint of moldability and heat resistance, it is composed of structural units derived from diamine and structural units derived from dicarboxylic acid, and 70 mol% or more of the structural units derived from diamine is xylylene. A semi-aromatic polyamide resin derived from an amine and having 70 mol% or more of the structural units derived from a dicarboxylic acid derived from an α,ω-straight-chain aliphatic dicarboxylic acid having 4 to 20 carbon atoms (hereinafter referred to as "XD-based polyamide" (sometimes) is preferred.

XD系ポリアミドは、ジアミン由来の構成単位の70モル%以上、好ましくは80モル%以上、より好ましくは90モル%以上、さらに好ましくは95モル%以上がキシリレンジアミンに由来し、ジカルボン酸由来の構成単位の70モル%以上、好ましくは80モル%以上、より好ましくは90モル%、さらに好ましくは95モル%以上が、炭素数が4~20のα,ω-直鎖脂肪族ジカルボン酸に由来する。
キシリレンジアミンは、パラキシリレンジアミン、メタキシリレンジアミン、または、両者の混合物が好ましく、少なくともメタキシリレンジアミンを含むことがより好ましい。
In the XD-based polyamide, 70 mol% or more, preferably 80 mol% or more, more preferably 90 mol% or more, and still more preferably 95 mol% or more of the diamine-derived structural units are derived from xylylenediamine, and dicarboxylic acid-derived 70 mol% or more, preferably 80 mol% or more, more preferably 90 mol%, and still more preferably 95 mol% or more of the structural units are derived from α,ω-linear aliphatic dicarboxylic acid having 4 to 20 carbon atoms do.
The xylylenediamine is preferably para-xylylenediamine, meta-xylylenediamine, or a mixture of both, and more preferably includes at least meta-xylylenediamine.

XD系ポリアミドの原料ジアミン成分として用いることができるメタキシリレンジアミンおよびパラキシリレンジアミン以外のジアミンとしては、テトラメチレンジアミン、ペンタメチレンジアミン、2-メチルペンタンジアミン、ヘキサメチレンジアミン、ヘプタメチレンジアミン、オクタメチレンジアミン、ノナメチレンジアミン、デカメチレンジアミン、ドデカメチレンジアミン、2,2,4-トリメチル-ヘキサメチレンジアミン、2,4,4-トリメチルヘキサメチレンジアミン等の脂肪族ジアミン、1,3-ビス(アミノメチル)シクロヘキサン、1,4-ビス(アミノメチル)シクロヘキサン、1,3-ジアミノシクロヘキサン、1,4-ジアミノシクロヘキサン、ビス(4-アミノシクロヘキシル)メタン、2,2-ビス(4-アミノシクロヘキシル)プロパン、ビス(アミノメチル)デカリン、ビス(アミノメチル)トリシクロデカン等の脂環式ジアミン、ビス(4-アミノフェニル)エーテル、パラフェニレンジアミン、ビス(アミノメチル)ナフタレン等の芳香環を有するジアミン等を例示することができ、1種または2種以上を混合して使用できる。
ジアミン成分として、キシリレンジアミン以外のジアミンを用いる場合は、ジアミン由来の構成単位の20モル%未満であることが好ましく、10モル%以下であることがより好ましい。
Examples of diamines other than meta-xylylenediamine and para-xylylenediamine that can be used as raw material diamine components for XD-based polyamides include tetramethylenediamine, pentamethylenediamine, 2-methylpentanediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, and octamethylenediamine. Aliphatic diamines such as methylenediamine, nonamethylenediamine, decamethylenediamine, dodecamethylenediamine, 2,2,4-trimethyl-hexamethylenediamine, 2,4,4-trimethylhexamethylenediamine, 1,3-bis(amino methyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1,3-diaminocyclohexane, 1,4-diaminocyclohexane, bis(4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane , alicyclic diamines such as bis(aminomethyl)decalin and bis(aminomethyl)tricyclodecane, diamines having aromatic rings such as bis(4-aminophenyl) ether, paraphenylenediamine, bis(aminomethyl)naphthalene, etc. can be exemplified, and can be used alone or in combination of two or more.
When a diamine other than xylylenediamine is used as the diamine component, it is preferably less than 20 mol %, more preferably 10 mol % or less, of the constituent units derived from the diamine.

半芳香族ポリアミド樹脂の原料ジカルボン酸成分として用いるのに好ましい炭素数4~20のα,ω-直鎖脂肪族ジカルボン酸としては、例えばコハク酸、グルタル酸、ピメリン酸、スベリン酸、アゼライン酸、アジピン酸、セバシン酸、ウンデカン二酸、ドデカン二酸等の脂肪族ジカルボン酸が例示でき、1種または2種以上を混合して使用できるが、これらの中でも半芳香族ポリアミド樹脂の融点が成形加工するのに適切な範囲となることから、アジピン酸またはセバシン酸が好ましく、アジピン酸がより好ましい。 Examples of α,ω-straight-chain aliphatic dicarboxylic acids having 4 to 20 carbon atoms that are preferable for use as the starting dicarboxylic acid component of the semiaromatic polyamide resin include succinic acid, glutaric acid, pimelic acid, suberic acid, azelaic acid, Aliphatic dicarboxylic acids such as adipic acid, sebacic acid, undecanedioic acid, and dodecanedioic acid can be exemplified, and one or a mixture of two or more thereof can be used. Adipic acid or sebacic acid is preferred, and adipic acid is more preferred, since it is in a range suitable for

上記炭素数4~20のα,ω-直鎖脂肪族ジカルボン酸以外のジカルボン酸成分としては、イソフタル酸、テレフタル酸、オルソフタル酸等のフタル酸化合物、1,2-ナフタレンジカルボン酸、1,3-ナフタレンジカルボン酸、1,4-ナフタレンジカルボン酸、1,5-ナフタレンジカルボン酸、1,6-ナフタレンジカルボン酸、1,7-ナフタレンジカルボン酸、1,8-ナフタレンジカルボン酸、2,3-ナフタレンジカルボン酸、2,6-ナフタレンジカルボン酸、2,7-ナフタレンジカルボン酸といった異性体等のナフタレンジカルボン酸等を例示することができ、1種または2種以上を混合して使用できる。炭素数4~20のα,ω-直鎖脂肪族ジカルボン酸以外のジカルボン酸成分を用いる場合、ジカルボン酸由来の構成単位の20モル%未満であることが好ましく、10モル%以下であることがより好ましい。 Examples of dicarboxylic acid components other than the α,ω-straight-chain aliphatic dicarboxylic acids having 4 to 20 carbon atoms include phthalic acid compounds such as isophthalic acid, terephthalic acid and orthophthalic acid, 1,2-naphthalenedicarboxylic acid, 1,3 -naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 1,6-naphthalenedicarboxylic acid, 1,7-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid, 2,3-naphthalene Naphthalenedicarboxylic acids such as isomers such as dicarboxylic acids, 2,6-naphthalenedicarboxylic acid and 2,7-naphthalenedicarboxylic acid can be exemplified, and can be used singly or in combination of two or more. When using a dicarboxylic acid component other than the α,ω-straight-chain aliphatic dicarboxylic acid having 4 to 20 carbon atoms, it is preferably less than 20 mol% of the structural units derived from the dicarboxylic acid, and is preferably 10 mol% or less. more preferred.

尚、半芳香族ポリアミド樹脂は、ジアミン由来の構成単位とジカルボン酸由来の構成単位を主成分として構成されるが、これら以外の構成単位を完全に排除するものではなく、ε-カプロラクタムやラウロラクタム等のラクタム類、アミノカプロン酸、アミノウンデカン酸等の脂肪族アミノカルボン酸類由来の構成単位を含んでいてもよいことは言うまでもない。本発明では、半芳香族ポリアミド樹脂におけるジアミン由来の構成単位とジカルボン酸由来の構成単位の合計は、全構成単位の90%以上を占めることが好ましく、95%以上を占めることがより好ましい。 The semi-aromatic polyamide resin is mainly composed of diamine-derived structural units and dicarboxylic acid-derived structural units, but does not completely exclude structural units other than these. It goes without saying that structural units derived from aliphatic aminocarboxylic acids such as lactams such as lactams such as aminocaproic acid and aminoundecanoic acid may be included. In the present invention, the sum of diamine-derived structural units and dicarboxylic acid-derived structural units in the semi-aromatic polyamide resin preferably accounts for 90% or more, more preferably 95% or more, of all structural units.

半芳香族ポリアミド樹脂の融点は、150~350℃であることが好ましく、180~330℃であることがより好ましく、200~300℃であることがさらに好ましい。
また、半芳香族ポリアミド樹脂のガラス転移温度は、50~150℃が好ましく、55~120℃がより好ましく、特に好ましくは60~100℃である。この範囲であると、成形品の耐熱性がより良好となる傾向にある。
The melting point of the semi-aromatic polyamide resin is preferably 150 to 350°C, more preferably 180 to 330°C, even more preferably 200 to 300°C.
Also, the glass transition temperature of the semi-aromatic polyamide resin is preferably 50 to 150°C, more preferably 55 to 120°C, and particularly preferably 60 to 100°C. Within this range, the heat resistance of the molded product tends to be better.

半芳香族ポリアミド樹脂の融点は、DSC(示差走査熱量測定)法により観測される昇温時の吸熱ピークのピークトップの温度として測定する。半芳香族ポリアミド樹脂のガラス転移温度は、半芳香族ポリアミド樹脂を一度加熱溶融させ熱履歴による結晶性への影響をなくした後、再度昇温して測定されるピークトップの温度として測定する。
具体的には、DSC測定器を用い、試料である半芳香族ポリアミド樹脂の量は約1mgとし、雰囲気ガスとしては窒素を30mL/分で流し、昇温速度は10℃/分の条件で、室温から予想される融点以上の温度まで加熱し溶融させた際に観測される吸熱ピークのピークトップの温度から融点を求める。次いで、溶融した半芳香族ポリアミド樹脂を、ドライアイスで急冷し、10℃/分の速度で融点以上の温度まで再度昇温し、ガラス転移温度を求める。DSC測定器としては、島津製作所(SHIMADZU CORPORATION)製、DSC-60が挙げられる。
The melting point of the semi-aromatic polyamide resin is measured as the peak top temperature of the endothermic peak during temperature rise observed by DSC (differential scanning calorimetry). The glass transition temperature of the semi-aromatic polyamide resin is measured as the peak top temperature obtained by once heating and melting the semi-aromatic polyamide resin to eliminate the influence of the heat history on the crystallinity, and then raising the temperature again.
Specifically, using a DSC measuring instrument, the amount of the semi-aromatic polyamide resin as a sample was about 1 mg, nitrogen was flowed at 30 mL / min as the atmosphere gas, and the temperature increase rate was 10 ° C. / min. The melting point is determined from the peak top temperature of the endothermic peak observed when the material is melted by heating from room temperature to a temperature higher than the expected melting point. Next, the molten semi-aromatic polyamide resin is rapidly cooled with dry ice, heated again to a temperature above the melting point at a rate of 10° C./min, and the glass transition temperature is determined. The DSC measuring instrument includes DSC-60 manufactured by SHIMADZU CORPORATION.

半芳香族ポリアミド樹脂は、数平均分子量(Mn)が6,000~30,000であることが好ましく、より好ましくは8,000~28,000であり、さらに好ましくは9,000~26,000であり、一層好ましくは10,000~24,000であり、より一層好ましくは11,000~22,000である。このような範囲であると、耐熱性、弾性率、寸法安定性、成形加工性がより良好となる。 The semi-aromatic polyamide resin preferably has a number average molecular weight (Mn) of 6,000 to 30,000, more preferably 8,000 to 28,000, still more preferably 9,000 to 26,000. , more preferably 10,000 to 24,000, and even more preferably 11,000 to 22,000. Within such a range, heat resistance, elastic modulus, dimensional stability, and moldability are improved.

なお、ここでいう数平均分子量(Mn)とは、半芳香族ポリアミド樹脂の末端アミノ基濃度[NH2](μ当量/g)と末端カルボキシル基濃度[COOH](μ当量/g)から、次式で算出される。
数平均分子量(Mn)=2,000,000/([COOH]+[NH2])
The number average molecular weight (Mn) referred to here is defined by the terminal amino group concentration [NH 2 ] (μ equivalent/g) and the terminal carboxyl group concentration [COOH] (μ equivalent/g) of the semi-aromatic polyamide resin. It is calculated by the following formula.
Number average molecular weight (Mn) = 2,000,000/([COOH] + [ NH2 ])

半芳香族ポリアミド樹脂は、分子量分布(重量平均分子量/数平均分子量(Mw/Mn))が、好ましくは1.8~3.1である。分子量分布は、より好ましくは1.9~3.0、さらに好ましくは2.0~2.9である。分子量分布をこのような範囲とすることにより、機械的物性に優れた立体構造物が得られやすい傾向にある。
半芳香族ポリアミド樹脂の分子量分布は、例えば、重合時に使用する開始剤や触媒の種、量および反応温度、圧力、時間等の重合反応条件などを適宜選択することにより調整できる。また、異なる重合条件によって得られた平均分子量の異なる複数種の半芳香族ポリアミド樹脂を混合したり、重合後の半芳香族ポリアミド樹脂を分別沈殿させることにより調整することもできる。
The semi-aromatic polyamide resin preferably has a molecular weight distribution (weight average molecular weight/number average molecular weight (Mw/Mn)) of 1.8 to 3.1. The molecular weight distribution is more preferably 1.9-3.0, more preferably 2.0-2.9. By setting the molecular weight distribution within such a range, there is a tendency to easily obtain a three-dimensional structure having excellent mechanical properties.
The molecular weight distribution of the semi-aromatic polyamide resin can be adjusted, for example, by appropriately selecting the species and amounts of initiators and catalysts used during polymerization and polymerization reaction conditions such as reaction temperature, pressure and time. It can also be prepared by mixing a plurality of types of semi-aromatic polyamide resins with different average molecular weights obtained under different polymerization conditions, or by separating and precipitating the semi-aromatic polyamide resins after polymerization.

分子量分布は、GPC測定により求めることができ、具体的には、装置として東ソー社製「HLC-8320GPC」、カラムとして、東ソー社製「TSK gel Super HM-H」2本を使用し、溶離液として、トリフルオロ酢酸ナトリウム濃度10mmol/Lのヘキサフルオロイソプロパノール(HFIP)、樹脂濃度0.02質量%、カラム温度40℃、流速0.3mL/分、屈折率検出器(RI)の条件で測定し、標準ポリメチルメタクリレート(PMMA)換算の値として求めることができる。また、検量線は6水準のPMMAをHFIPに溶解させて測定し作成する。 The molecular weight distribution can be determined by GPC measurement, specifically, as an apparatus "HLC-8320GPC" manufactured by Tosoh Corporation, as a column, two "TSK gel Super HM-H" manufactured by Tosoh Corporation are used, and an eluent is used. As, hexafluoroisopropanol (HFIP) with a sodium trifluoroacetate concentration of 10 mmol / L, a resin concentration of 0.02% by mass, a column temperature of 40 ° C., a flow rate of 0.3 mL / min, and a refractive index detector (RI). , can be obtained as a value in terms of standard polymethyl methacrylate (PMMA). A calibration curve is prepared by dissolving 6 levels of PMMA in HFIP and measuring.

本発明の成形品における半芳香族ポリアミド樹脂の含有量の下限は、25質量%以上であることが好ましく、30質量%以上であることがより好ましく、40質量%以上であることがさらに好ましく、50質量%以上であることが一層好ましく、55質量%以上であることがより一層好ましい。前記含有量の上限は、75質量%以下であることが好ましく、70質量%以下であることがより好ましい。
本発明の成形品は、半芳香族ポリアミド樹脂を1種のみ含んでいてもよいし、2種以上含んでいてもよい。2種以上含む場合、合計量が上記範囲となることが好ましい。
The lower limit of the content of the semi-aromatic polyamide resin in the molded article of the present invention is preferably 25% by mass or more, more preferably 30% by mass or more, and further preferably 40% by mass or more. It is more preferably 50% by mass or more, and even more preferably 55% by mass or more. The upper limit of the content is preferably 75% by mass or less, more preferably 70% by mass or less.
The molded article of the present invention may contain only one type of semi-aromatic polyamide resin, or may contain two or more types. When two or more types are included, the total amount is preferably within the above range.

本発明の成形品は、半芳香族ポリアミド樹脂と後述する繊維を含むフィラーの合計が全体の90質量%以上を占めることが好ましい。 In the molded article of the present invention, the total amount of the semi-aromatic polyamide resin and the filler containing fibers described below preferably accounts for 90% by mass or more of the entirety.

<他のポリアミド樹脂>
本発明の成形品は、上記半芳香族ポリアミド樹脂以外のポリアミド樹脂を1種または2種以上含んでいてもよい。このようなポリアミド樹脂としては、ポリアミド4、ポリアミド6、ポリアミド11、ポリアミド12、ポリアミド46、ポリアミド66、ポリアミド610、ポリアミド612等が挙げられる。
もちろん、本発明では、これらの他のポリアミド樹脂は実質的に含まない構成であってもよい。実質的に含まないとは、他のポリアミド樹脂の含有量が、本発明の成形品に含まれる半芳香族ポリアミド樹脂の含有量の2質量%以下であることをいい、1質量%以下が好ましく、0.1質量%以下がより好ましい。
<Other polyamide resins>
The molded article of the present invention may contain one or more polyamide resins other than the semi-aromatic polyamide resin. Such polyamide resins include polyamide 4, polyamide 6, polyamide 11, polyamide 12, polyamide 46, polyamide 66, polyamide 610, polyamide 612 and the like.
Of course, in the present invention, the configuration may be such that these other polyamide resins are not substantially included. "Substantially free" means that the content of the other polyamide resin is 2% by mass or less of the content of the semi-aromatic polyamide resin contained in the molded article of the present invention, preferably 1% by mass or less. , 0.1% by mass or less is more preferable.

<繊維>
本発明の成形品は、繊維を含む。
繊維は、数平均繊維長が300μmを超えるものであれば特に定めるものではなく、公知の繊維を用いることができる。繊維の数平均繊維長の下限は、500μm以上が好ましく、1.0mm以上がより好ましく、2.0mm以上がさらに好ましく、3.0mm以上が一層好ましい。繊維の数平均繊維長の上限は、6.0mm以下が好ましく、5.0mm以下がより好ましく、4.0mm以下がさらに好ましい。
<Fiber>
The molded article of the present invention contains fibers.
The fibers are not particularly limited as long as the number average fiber length exceeds 300 μm, and known fibers can be used. The lower limit of the number average fiber length of the fibers is preferably 500 μm or longer, more preferably 1.0 mm or longer, even more preferably 2.0 mm or longer, and still more preferably 3.0 mm or longer. The upper limit of the number average fiber length of the fibers is preferably 6.0 mm or less, more preferably 5.0 mm or less, and even more preferably 4.0 mm or less.

繊維の種類は特に限定されないが、ガラス繊維、炭素繊維、植物繊維(ケナフ(Kenaf)、竹繊維等を含む)、アルミナ繊維、ボロン繊維、セラミック繊維、金属繊維(スチール繊維等)等の無機繊維、および、アラミド繊維、ポリオキシメチレン繊維、ポリパラフェニレンベンゾビスオキサゾール繊維、超高分子量ポリエチレン繊維等の有機繊維などが挙げられる。なかでも、炭素繊維、アラミド繊維およびガラス繊維から選択される少なくとも1種であることが好ましく、炭素繊維およびガラス繊維から選択される少なくとも1種であることがより好ましく、ガラス繊維から選択される少なくとも1種であることがさらに好ましい。 The type of fiber is not particularly limited, but inorganic fibers such as glass fiber, carbon fiber, vegetable fiber (including kenaf, bamboo fiber, etc.), alumina fiber, boron fiber, ceramic fiber, metal fiber (steel fiber, etc.). , and organic fibers such as aramid fibers, polyoxymethylene fibers, polyparaphenylenebenzobisoxazole fibers, and ultra-high molecular weight polyethylene fibers. Among them, it is preferably at least one selected from carbon fiber, aramid fiber and glass fiber, more preferably at least one selected from carbon fiber and glass fiber, and at least one selected from glass fiber. One type is more preferable.

ガラス繊維は、Aガラス、Cガラス、Eガラス、Sガラスなどのガラス組成を有し、特に、Eガラス(無アルカリガラス)が好ましい。ガラス繊維は、1種のみ含んでいてもよいし、2種以上含んでいてもよい。 The glass fiber has a glass composition such as A glass, C glass, E glass, S glass, etc. E glass (alkali-free glass) is particularly preferable. Only one kind of glass fiber may be contained, or two or more kinds thereof may be contained.

本発明で用いる繊維は、単繊維または単繊維を複数本撚り合わせたものであってもよい。
本発明で用いる繊維は、表面処理剤および集束剤の少なくとも一方で処理されていることが好ましい。表面処理剤としては、シラン系カップリング剤、チタン系カップリング剤、およびアルミネート系カップリング剤等のカップリング剤が例示される。集束剤としては、エポキシ系化合物、ウレタン系化合物、カルボン酸系化合物、ウレタン/マレイン酸変性化合物およびウレタン/アミン変性系化合物が例示される。表面処理剤および/または集束剤を用いることにより、半芳香族ポリアミド樹脂との密着性をより向上させ、本発明の成形品の機械的強度をより向上させることができる。
The fiber used in the present invention may be a single fiber or a plurality of twisted single fibers.
The fibers used in the present invention are preferably treated with at least one of a surface treatment agent and a sizing agent. Examples of surface treatment agents include coupling agents such as silane-based coupling agents, titanium-based coupling agents, and aluminate-based coupling agents. Examples of sizing agents include epoxy-based compounds, urethane-based compounds, carboxylic acid-based compounds, urethane/maleic acid-modified compounds, and urethane/amine-modified compounds. By using a surface treatment agent and/or a sizing agent, the adhesion to the semi-aromatic polyamide resin can be further improved, and the mechanical strength of the molded article of the present invention can be further improved.

本発明で用いる繊維の含有量の下限は、25質量%以上であることが好ましく、26質量%以上であることがより好ましく、28質量%以上であることがさらに好ましい。前記含有量の上限は、75質量%以下であることが好ましく、65質量%以下であることがより好ましく、55質量%以下であることがさらに好ましく、45質量%以下であることが一層好ましく、35質量%以下であることがより一層好ましい。
本発明の成形品は、繊維を1種のみ含んでいてもよいし、2種以上含んでいてもよい。2種以上含む場合は、合計量が上記範囲となることが好ましい。
The lower limit of the content of the fibers used in the present invention is preferably 25% by mass or more, more preferably 26% by mass or more, and even more preferably 28% by mass or more. The upper limit of the content is preferably 75% by mass or less, more preferably 65% by mass or less, further preferably 55% by mass or less, and even more preferably 45% by mass or less, It is more preferably 35% by mass or less.
The molded article of the present invention may contain only one type of fiber, or may contain two or more types. When two or more kinds are included, the total amount is preferably within the above range.

<他のフィラー>
本発明の成形品は、上記数平均繊維長が300μmを超える繊維に加え、他のフィラーを含んでいてもよい。他のフィラーとしては、数平均繊維長が300μm以下の繊維が挙げられる。
また、本発明の成形品は、上記数平均繊維長が300μmを超える繊維以外のフィラーの含有量が、上記数平均繊維長が300μmを超える繊維の10質量%以下であることが好ましく、5質量%以下であることがより好ましく、3質量%以下であることがさらに好ましく、1質量%以下であることが一層好ましい。このような範囲とすることにより、本発明の効果がより効果的に発揮される傾向にある。
<Other fillers>
The molded article of the present invention may contain other fillers in addition to the fibers having a number average fiber length exceeding 300 μm. Other fillers include fibers having a number average fiber length of 300 μm or less.
In addition, in the molded article of the present invention, the content of filler other than the fibers having a number average fiber length exceeding 300 μm is preferably 10% by mass or less of the fibers having a number average fiber length exceeding 300 μm, and 5 mass % or less, more preferably 3 mass % or less, and even more preferably 1 mass % or less. By setting it as such a range, there exists a tendency for the effect of this invention to be exhibited more effectively.

<黒色着色剤>
本発明の成形品は、黒色着色剤を含んでいてもよい。黒色着色剤を配合することにより、遮光性に優れた成形品が得られる。
本発明で用いる黒色着色剤としては、カーボンブラックが例示される。カーボンブラックの詳細は、特開2011-57977号公報の段落0021の記載を参酌でき、これらの内容は本明細書に組み込まれる。
また、本発明の成形品にカーボンブラック等の黒色着色剤を配合する場合、マスターバッチを形成してから、半芳香族ポリアミド樹脂と混練することが好ましい。マスターバッチの詳細については、特開2011-57977号公報の段落0038~0042の記載を参酌でき、これらの内容は本明細書に組み込まれる。
さらに、本発明の成形品をレーザー溶着で製造する場合、光透過性の黒色着色剤を用いることも好ましい。光透過性の黒色着色剤としては、照射するレーザー光波長の範囲、例えば、波長800nm~1064nmの範囲において透過率の高い着色剤である。具体的には、ニグロシン、ナフタロシアニン、アニリンブラック、フタロシアニン、ポルフィリン、ペリレン、ペリノン、クオテリレン、アゾ染料、アントラキノン、スクエア酸誘導体、およびインモニウム染料等が挙げられる。市販品としては、オリエント化学工業社製の着色剤であるe-Bind ACW-9871、e-BIND LTW-8731H等が例示される。
本発明の成形品が黒色着色剤を含む場合、その含有量は、半芳香族ポリアミド樹脂100質量部に対し、0.1~10質量部であることが好ましく、0.5~8質量部がより好ましく、1~6質量部がさらに好ましい。
本発明の成形品は、黒色着色剤を、1種のみ含んでいてもよいし、2種以上含んでいてもよい。2種以上含む場合、合計量が上記範囲となることが好ましい。
<Black colorant>
The molded article of the present invention may contain a black colorant. By blending a black colorant, a molded article having excellent light-shielding properties can be obtained.
Carbon black is exemplified as the black colorant used in the present invention. Details of carbon black can be referred to the description in paragraph 0021 of JP-A-2011-57977, and the contents thereof are incorporated herein.
Further, when a black colorant such as carbon black is blended into the molded article of the present invention, it is preferable to knead it with the semi-aromatic polyamide resin after forming a masterbatch. For details of the masterbatch, reference can be made to paragraphs 0038 to 0042 of JP-A-2011-57977, the contents of which are incorporated herein.
Furthermore, when producing the molded article of the present invention by laser welding, it is also preferable to use a light-transmitting black colorant. The light-transmissive black colorant is a colorant with high transmittance in the wavelength range of the irradiated laser light, for example, the wavelength range of 800 nm to 1064 nm. Specific examples include nigrosine, naphthalocyanine, aniline black, phthalocyanine, porphyrin, perylene, perinone, quaterrylene, azo dyes, anthraquinone, squaric acid derivatives, and immonium dyes. Examples of commercially available products include e-Bind ACW-9871 and e-BIND LTW-8731H, which are colorants manufactured by Orient Chemical Industry Co., Ltd.
When the molded article of the present invention contains a black colorant, its content is preferably 0.1 to 10 parts by mass, and 0.5 to 8 parts by mass with respect to 100 parts by mass of the semi-aromatic polyamide resin. More preferably, 1 to 6 parts by mass is even more preferable.
The molded article of the present invention may contain only one kind of black colorant, or may contain two or more kinds thereof. When two or more types are included, the total amount is preferably within the above range.

<タルク>
本発明の成形品はタルクを含んでいてもよい。本発明では、タルクを配合することにより、結晶化を促進することができる。
本発明の成形品における、タルクの配合量は、成形品に対し、0.05~20質量%であることが好ましく、0.1~10質量%であることがより好ましく、0.15~5質量%であることがさらに好ましく、0.2~2質量%であることが一層好ましい。タルクは、1種のみを用いてもよいし、2種以上を併用してもよい。2種以上の場合は、合計量が上記範囲となることが好ましい。
<Talc>
Molded articles of the present invention may contain talc. In the present invention, crystallization can be promoted by blending talc.
The amount of talc compounded in the molded article of the present invention is preferably 0.05 to 20% by mass, more preferably 0.1 to 10% by mass, and more preferably 0.15 to 5% by mass. % by mass is more preferred, and 0.2 to 2% by mass is even more preferred. Only one type of talc may be used, or two or more types may be used in combination. When two or more kinds are used, the total amount is preferably within the above range.

本発明では、特に、黒色着色剤とタルクを含み、前記成形品における、黒色着色剤とタルクの質量比(黒色着色剤/タルク)が1.5~2.5であることが好ましく、1.8~2.2であることがより好ましい。このような範囲とすることにより、半芳香族ポリアミド樹脂の結晶化を促進しつつ、遮光性に優れた成形品が得られる。 In the present invention, it is particularly preferable that a black coloring agent and talc are included, and the mass ratio of the black coloring agent and talc (black coloring agent/talc) in the molded article is 1.5 to 2.5. It is more preferably 8 to 2.2. Such a range promotes the crystallization of the semi-aromatic polyamide resin and provides a molded product with excellent light-shielding properties.

<離型剤>
本発明の成形品は、離型剤を含んでいてもよい。離型剤としては、例えば、脂肪族カルボン酸、脂肪族カルボン酸の塩、脂肪族カルボン酸とアルコールとのエステル、数平均分子量200~15,000の脂肪族炭化水素化合物、ポリシロキサン系シリコーンオイルなどが挙げられる。
<Release agent>
The molded article of the present invention may contain a release agent. Release agents include, for example, aliphatic carboxylic acids, salts of aliphatic carboxylic acids, esters of aliphatic carboxylic acids and alcohols, aliphatic hydrocarbon compounds having a number average molecular weight of 200 to 15,000, and polysiloxane-based silicone oils. etc.

脂肪族カルボン酸としては、例えば、飽和または不飽和の脂肪族一価、二価または三価カルボン酸を挙げることができる。ここで脂肪族カルボン酸とは、脂環式のカルボン酸も包含する。これらの中で好ましい脂肪族カルボン酸は炭素数6~36の一価または二価カルボン酸であり、炭素数6~36の脂肪族飽和一価カルボン酸がより好ましい。かかる脂肪族カルボン酸の具体例としては、パルミチン酸、ステアリン酸、カプロン酸、カプリン酸、ラウリン酸、アラキン酸、ベヘン酸、リグノセリン酸、セロチン酸、メリシン酸、テトラトリアコンタン酸、モンタン酸、アジピン酸、アゼライン酸などが挙げられる。また、脂肪族カルボン酸の塩としては、ナトリウム塩、カリウム塩、カルシウム塩、マグネシウム塩が例示される。 Aliphatic carboxylic acids include, for example, saturated or unsaturated aliphatic monovalent, divalent or trivalent carboxylic acids. Here, the aliphatic carboxylic acid also includes alicyclic carboxylic acid. Among these, preferred aliphatic carboxylic acids are monovalent or divalent carboxylic acids having 6 to 36 carbon atoms, more preferably aliphatic saturated monovalent carboxylic acids having 6 to 36 carbon atoms. Specific examples of such aliphatic carboxylic acids include palmitic acid, stearic acid, caproic acid, capric acid, lauric acid, arachidic acid, behenic acid, lignoceric acid, cerotic acid, melissic acid, tetratriacontanoic acid, montanic acid, and adipine. acid, azelaic acid, and the like. Examples of salts of aliphatic carboxylic acids include sodium salts, potassium salts, calcium salts, and magnesium salts.

脂肪族カルボン酸とアルコールとのエステルにおける脂肪族カルボン酸としては、例えば、前記脂肪族カルボン酸と同じものが使用できる。一方、アルコールとしては、例えば、飽和または不飽和の一価または多価アルコールが挙げられる。これらのアルコールは、フッ素原子、アリール基などの置換基を有していてもよい。これらの中では、炭素数30以下の一価または多価の飽和アルコールが好ましく、炭素数30以下の脂肪族または脂環式飽和一価アルコールまたは脂肪族飽和多価アルコールがより好ましい。 As the aliphatic carboxylic acid in the ester of aliphatic carboxylic acid and alcohol, for example, the same aliphatic carboxylic acid as mentioned above can be used. Alcohols, on the other hand, include, for example, saturated or unsaturated monohydric or polyhydric alcohols. These alcohols may have substituents such as fluorine atoms and aryl groups. Among these, monohydric or polyhydric saturated alcohols having 30 or less carbon atoms are preferable, and aliphatic or alicyclic saturated monohydric alcohols or saturated aliphatic polyhydric alcohols having 30 or less carbon atoms are more preferable.

かかるアルコールの具体例としては、オクタノール、デカノール、ドデカノール、ステアリルアルコール、ベヘニルアルコール、エチレングリコール、ジエチレングリコール、グリセリン、ペンタエリスリトール、2,2-ジヒドロキシペルフルオロプロパノール、ネオペンチレングリコール、ジトリメチロールプロパン、ジペンタエリスリトール等が挙げられる。 Specific examples of such alcohols include octanol, decanol, dodecanol, stearyl alcohol, behenyl alcohol, ethylene glycol, diethylene glycol, glycerin, pentaerythritol, 2,2-dihydroxyperfluoropropanol, neopentylene glycol, ditrimethylolpropane, dipentaerythritol, and the like. are mentioned.

脂肪族カルボン酸とアルコールとのエステルの具体例としては、蜜ロウ(ミリシルパルミテートを主成分とする混合物)、ステアリン酸ステアリル、ベヘン酸ベヘニル、ベヘン酸ステアリル、グリセリンモノパルミテート、グリセリンモノステアレート、グリセリンジステアレート、グリセリントリステアレート、ペンタエリスリトールモノパルミテート、ペンタエリスリトールモノステアレート、ペンタエリスリトールジステアレート、ペンタエリスリトールトリステアレート、ペンタエリスリトールテトラステアレート等が挙げられる。 Specific examples of esters of aliphatic carboxylic acids and alcohols include beeswax (a mixture containing myricyl palmitate as a main component), stearyl stearate, behenyl behenate, stearyl behenate, glycerin monopalmitate, glycerin monostea glycerin distearate, glycerin tristearate, pentaerythritol monopalmitate, pentaerythritol monostearate, pentaerythritol distearate, pentaerythritol tristearate, pentaerythritol tetrastearate and the like.

数平均分子量200~15,000の脂肪族炭化水素としては、例えば、流動パラフィン、パラフィンワックス、マイクロワックス、ポリエチレンワックス、フィッシャ-トロプシュワックス、炭素数3~12のα-オレフィンオリゴマー等が挙げられる。なお、ここで脂肪族炭化水素としては、脂環式炭化水素も含まれる。また、脂肪族炭化水素の数平均分子量は好ましくは5,000以下である。
これらの中では、パラフィンワックス、ポリエチレンワックスまたはポリエチレンワックスの部分酸化物が好ましく、パラフィンワックス、ポリエチレンワックスがより好ましい。
Examples of aliphatic hydrocarbons having a number average molecular weight of 200 to 15,000 include liquid paraffin, paraffin wax, microwax, polyethylene wax, Fischer-Tropsch wax, and α-olefin oligomers having 3 to 12 carbon atoms. In addition, an alicyclic hydrocarbon is also contained as an aliphatic hydrocarbon here. Also, the number average molecular weight of the aliphatic hydrocarbon is preferably 5,000 or less.
Among these, paraffin wax, polyethylene wax, or partial oxides of polyethylene wax are preferable, and paraffin wax and polyethylene wax are more preferable.

本発明の成形品が離型剤を含む場合、離型剤の含有量は、成形品に対し、0.001~2質量%であることが好ましく、0.01~1質量%であることがより好ましい。離型剤は、1種のみでもよいし、2種以上含んでいてもよい。2種以上含む場合は、合計量が上記範囲となることが好ましい。離型剤の含有量を上記範囲とすることにより、離型性の効果を十分に保ちつつ、耐加水分解性の低下を抑制し、さらに、射出成形時の金型汚染を効果的に抑制できる。 When the molded product of the present invention contains a mold release agent, the content of the mold release agent is preferably 0.001 to 2% by mass, more preferably 0.01 to 1% by mass, relative to the molded product. more preferred. Only one release agent may be used, or two or more release agents may be used. When two or more kinds are included, the total amount is preferably within the above range. By setting the content of the release agent within the above range, it is possible to suppress deterioration in hydrolysis resistance while sufficiently maintaining the effect of release properties, and to effectively suppress mold contamination during injection molding. .

<その他の添加剤>
本発明の成形品は、本発明の趣旨を損なわない範囲で、上記の他、ポリアミド樹脂に一般的に用いられうる他の添加剤を含んでいてもよい。このようなその他の添加剤としては、ポリアミド樹脂以外の樹脂、潤滑剤、安定剤、難燃剤、蛍光漂白剤、可塑化剤、酸化防止剤、紫外線吸収剤、帯電防止剤、流動性改良剤等が例示される。他の添加剤の含有量は、合計で、成形品の5質量%以下であることが好ましい。これらの添加剤の詳細は、特開2011-57977号公報や特開2015-129244号公報の記載を参酌でき、これらの内容は本明細書に組み込まれる。
他の樹脂としては、ポリエステル樹脂、ポリフェニレンスルフィド樹脂、ポリフェニレンエーテル樹脂、ポリカーボネート樹脂、ポリアリレート樹脂、フェノール樹脂、およびエポキシ樹脂等が挙げられる。
<Other additives>
The molded article of the present invention may contain other additives generally used in polyamide resins, in addition to the above, as long as the gist of the present invention is not impaired. Such other additives include resins other than polyamide resins, lubricants, stabilizers, flame retardants, fluorescent bleaches, plasticizers, antioxidants, ultraviolet absorbers, antistatic agents, fluidity improvers, and the like. is exemplified. The total content of other additives is preferably 5% by mass or less of the molded product. Details of these additives can be referred to JP-A-2011-57977 and JP-A-2015-129244, the contents of which are incorporated herein.
Other resins include polyester resins, polyphenylene sulfide resins, polyphenylene ether resins, polycarbonate resins, polyarylate resins, phenolic resins, epoxy resins, and the like.

本発明の成形品を構成するポリアミド樹脂組成物は、1mmの厚さに成形し、40℃、相対湿度90%の条件下に42時間静置した後の水分透過係数が3.0g・mm/day・m2以下であることが好ましく、1.5g・mm/day・m2以下であることがより好ましい。上記水分透過係数の下限値は0g・mm/day・m2であることが好ましいが、0.2g・mm/day・m2以上でも十分に実用レベルである。上記水分透過係数は、実施例に記載の方法で測定した値とする。
尚、ポリアミド樹脂の吸水率が低くても、水分透過係数が小さいとは言えない。これは、ポリアミド樹脂では、吸水速度と拡散速度が異なるためである。
The polyamide resin composition constituting the molded article of the present invention is molded to a thickness of 1 mm and has a moisture permeability coefficient of 3.0 g mm / It is preferably day·m 2 or less, more preferably 1.5 g·mm/day·m 2 or less. The lower limit of the water permeability coefficient is preferably 0 g·mm/day·m 2 , but 0.2 g·mm/day·m 2 or more is sufficiently practical. The water permeability coefficient is a value measured by the method described in Examples.
Incidentally, even if the water absorption of the polyamide resin is low, it cannot be said that the water permeability coefficient is small. This is because polyamide resins have different water absorption speeds and diffusion speeds.

本発明の成形品は、透明部材を有する各種保存容器、電気電子機器部品、オフィスオートメート(OA)機器部品、家電機器部品、機械機構部品、車両機構部品などに適用できる。特に、カメラ部品として好ましく用いられる。カメラ部品としては、バレルやホルダ、筐体、として用いられる。特に、本発明の成形品は、車載カメラのカメラ部品として好ましく用いられる。
本発明の成形品がカメラ部品の場合、最大長さが15~40mmであることが好ましい。このような構成とすることにより、性能と外観のバランスを備えたカメラ部品とすることができる。
本発明の成形品がカメラ部品の場合、前記ポリアミド樹脂組成物に由来する部材を含み、前記部材の割合が、1~99質量%であることが好ましい。このような構成とすることにより、カメラ部品の軽量化と、カメラ部品の強度のバランスに優れた成形品とすることができる。
特に、本発明の成形品は、射出成形品であることが好ましい。もちろん、本発明の成形品が射出成形品以外の成形品であってもよいことは言うまでもない。
The molded article of the present invention can be applied to various storage containers having transparent members, electric and electronic equipment parts, office automation (OA) equipment parts, household appliance parts, machine mechanism parts, vehicle mechanism parts, and the like. In particular, it is preferably used as a camera component. As camera parts, they are used as barrels, holders, and housings. In particular, the molded article of the present invention is preferably used as a camera component for a vehicle-mounted camera.
When the molded article of the present invention is a camera part, the maximum length is preferably 15-40 mm. With such a configuration, a camera component having a balance between performance and appearance can be obtained.
When the molded article of the present invention is a camera part, it preferably contains a member derived from the polyamide resin composition, and the proportion of the member is 1 to 99% by mass. With such a configuration, it is possible to reduce the weight of the camera component and to obtain a molded product having an excellent balance between the strength of the camera component.
In particular, the molded article of the present invention is preferably an injection molded article. Of course, it goes without saying that the molded article of the present invention may be a molded article other than an injection molded article.

次に、本発明の成形品の製造方法について、説明する。
本発明の成形品の製造方法は、半芳香族ポリアミド樹脂と、数平均繊維長が300μmを超える繊維を含み、前記半芳香族ポリアミド樹脂の末端カルボキシル基濃度が末端アミノ基濃度よりも高い、ポリアミド樹脂組成物を射出成形することを含む。半芳香族ポリアミド樹脂、繊維等の詳細は、上述と同様である。
射出成形時の温度は、260~300℃であることが好ましい。
本発明において、ポリアミド樹脂組成物の製造方法は、特に定めるものではなく、公知の熱可塑性樹脂組成物の製造方法を広く採用できる。具体的には、各成分を、タンブラーやヘンシェルミキサーなどの各種混合機を用い予め混合した後、バンバリーミキサー、ロール、ブラベンダー、単軸押出機、二軸押出機、ニーダーなどで溶融混練することによってポリアミド樹脂組成物を製造することができる。
Next, the method for manufacturing the molded product of the present invention will be described.
The method for producing a molded article of the present invention includes a semi-aromatic polyamide resin and a fiber having a number average fiber length of more than 300 μm, and the terminal carboxyl group concentration of the semi-aromatic polyamide resin is higher than the terminal amino group concentration. Including injection molding the resin composition. The details of the semi-aromatic polyamide resin, fibers, etc. are the same as described above.
The temperature during injection molding is preferably 260 to 300°C.
In the present invention, the method for producing the polyamide resin composition is not particularly defined, and widely known methods for producing thermoplastic resin compositions can be employed. Specifically, each component is mixed in advance using various mixers such as a tumbler and Henschel mixer, and then melt-kneaded with a Banbury mixer, roll, Brabender, single screw extruder, twin screw extruder, kneader, etc. A polyamide resin composition can be produced by

また、例えば、各成分を予め混合せずに、または、一部の成分のみを予め混合し、フィーダーを用いて押出機に供給して溶融混練して、ポリアミド樹脂組成物を製造することもできる。
さらに、例えば、一部の成分を予め混合し押出機に供給して溶融混練することで得られる樹脂組成物をマスターバッチとし、このマスターバッチを再度残りの成分と混合し、溶融混練することによってポリアミド樹脂組成物を製造することもできる。
Further, for example, the polyamide resin composition can be produced without pre-mixing the respective components, or pre-mixing only some of the components, supplying the mixture to an extruder using a feeder, and melt-kneading it. .
Furthermore, for example, a resin composition obtained by pre-mixing some components, supplying them to an extruder, and melt-kneading them is used as a masterbatch, and this masterbatch is mixed again with the remaining components and melt-kneaded. Polyamide resin compositions can also be produced.

以下に実施例を挙げて本発明をさらに具体的に説明する。以下の実施例に示す材料、使用量、割合、処理内容、処理手順等は、本発明の趣旨を逸脱しない限り、適宜、変更することができる。従って、本発明の範囲は以下に示す具体例に限定されるものではない。 EXAMPLES The present invention will be described more specifically with reference to examples below. The materials, usage amounts, ratios, processing details, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the gist of the present invention. Accordingly, the scope of the present invention is not limited to the specific examples shown below.

<半芳香族ポリアミド樹脂>
(ポリアミド(MXD6)の合成)
特開2011-140620号公報の段落0038の記載に従い、メタキシリレンジアミンとアジピン酸を重縮合してなり、末端アミノ基濃度40μ当量/g、末端カルボキシル基濃度90μ当量/gである半芳香族ポリアミド樹脂を合成した。末端カルボキシル基濃度に対する末端アミノ基濃度の比([NH2]/[COOH])は、0.44であった。得られた半芳香族ポリアミド樹脂を、「MXD6」という。
<Semi-aromatic polyamide resin>
(Synthesis of Polyamide (MXD6))
According to the description in paragraph 0038 of JP-A-2011-140620, a semi-aromatic compound obtained by polycondensation of metaxylylenediamine and adipic acid and having a terminal amino group concentration of 40 μeq/g and a terminal carboxyl group concentration of 90 μeq/g A polyamide resin was synthesized. The ratio of terminal amino group concentration to terminal carboxyl group concentration ([NH 2 ]/[COOH]) was 0.44. The obtained semi-aromatic polyamide resin is called "MXD6".

(ポリアミド(MP6-1)の合成)
特許第5218705号の実施例2の記載に従い、メタキシリレンジアミンとパラキシリレンジアミンとアジピン酸を重縮合してなり、末端カルボキシル基濃度([COOH])が95μ当量/g、末端アミノ基濃度([NH2])が45μ当量/gの半芳香族ポリアミド樹脂を合成した([NH2]/[COOH]=0.47)。
(Synthesis of Polyamide (MP6-1))
According to the description of Example 2 of Japanese Patent No. 5218705, meta-xylylenediamine, para-xylylenediamine and adipic acid are polycondensed, and the terminal carboxyl group concentration ([COOH]) is 95 μeq/g, the terminal amino group concentration is A semi-aromatic polyamide resin with ([NH 2 ]) of 45 μeq/g was synthesized ([NH 2 ]/[COOH]=0.47).

(ポリアミド(MP6-2)の合成)
撹拌機、分縮器、全縮器、温度計、滴下ロート及び窒素導入管、ストランドダイを備えた反応容器に、精秤したアジピン酸8768.4g(60mol)、次亜リン酸ナトリウム一水和物(NaH2PO2・H2O)3.105g(ポリアミド樹脂中のリン原子濃度として50質量ppm)、酢酸ナトリウム1.61gを入れ、十分に窒素置換した後、窒素を内圧0.4MPaまで充填、さらに少量の窒素気流下で系内を撹拌しながら170℃まで加熱した。次亜リン酸ナトリウム一水和物/酢酸ナトリウムのモル比は0.67とした。
これにメタキシリレンジアミンとパラキシリレンジアミンの7:3(モル比)の混合ジアミン8,335g(61mol)を撹拌下に滴下し、生成する縮合水を系外へ除きながら系内を連続的に昇温した。混合キシリレンジアミンの滴下終了後、内温を260℃として20分間溶融重合反応を継続した。次いで、1分あたり0.01MPaの速度で内圧を大気圧に戻した。
その後、再び系内を窒素で加圧し、ストランドダイからポリマーを取り出して、これをペレット化し、約24kgのポリアミド樹脂(MP6-2)を得た。得られたペレットを80℃の除湿エアー(露点-40℃)で1時間乾燥した。得られたMP6-2は、末端カルボキシル基濃度([COOH])が37μ当量/g、末端アミノ基濃度([NH2])が89μ当量/gであった。
(Synthesis of Polyamide (MP6-2))
Accurately weighed 8768.4 g (60 mol) of adipic acid and sodium hypophosphite monohydrate were placed in a reaction vessel equipped with a stirrer, partial condenser, total condenser, thermometer, dropping funnel, nitrogen inlet tube, and strand die. 3.105 g of compound (NaH 2 PO 2 ·H 2 O) (50 mass ppm as phosphorus atom concentration in polyamide resin) and 1.61 g of sodium acetate were added, and after sufficient nitrogen substitution, nitrogen was added to the internal pressure of 0.4 MPa. After filling, the inside of the system was heated to 170° C. under a small amount of nitrogen stream while stirring. The sodium hypophosphite monohydrate/sodium acetate molar ratio was 0.67.
To this, 8,335 g (61 mol) of a mixed diamine of meta-xylylenediamine and para-xylylenediamine (7:3 (molar ratio)) was added dropwise with stirring. The temperature was raised to After the dropwise addition of the mixed xylylenediamine was completed, the internal temperature was set to 260° C. and the melt polymerization reaction was continued for 20 minutes. Then, the internal pressure was returned to atmospheric pressure at a rate of 0.01 MPa per minute.
Thereafter, the inside of the system was pressurized again with nitrogen, and the polymer was taken out from the strand die and pelletized to obtain about 24 kg of polyamide resin (MP6-2). The obtained pellets were dried with dehumidified air at 80°C (dew point -40°C) for 1 hour. The obtained MP6-2 had a terminal carboxyl group concentration ([COOH]) of 37 μeq/g and a terminal amino group concentration ([NH 2 ]) of 89 μeq/g.

<末端基濃度>
末端アミノ基濃度は、半芳香族ポリアミド樹脂0.5gを30mLのフェノール/メタノール(体積比で4:1)混合溶液に20~30℃で攪拌溶解し、0.01Nの塩酸で滴定して測定した。また、末端カルボキシル基濃度については、半芳香族ポリアミド樹脂0.1gを30mLのベンジルアルコールに200℃で溶解し、160℃~165℃の範囲でフェノールレッド溶液を0.1mL加えた。その溶液を、0.132gのKOHをベンジルアルコール200mLに溶解させた滴定液(KOH濃度として0.01mol/L)で滴定を行い、色の変化が黄~赤となり色の変化がなくなった時点を終点とすることで算出した。
末端基濃度の単位は、μ当量/gである。
<Terminal group concentration>
The terminal amino group concentration is measured by dissolving 0.5 g of a semi-aromatic polyamide resin in a mixed solution of 30 mL of phenol/methanol (4:1 by volume) with stirring at 20 to 30° C. and titrating with 0.01N hydrochloric acid. did. As for the terminal carboxyl group concentration, 0.1 g of a semi-aromatic polyamide resin was dissolved in 30 mL of benzyl alcohol at 200°C, and 0.1 mL of phenol red solution was added in the range of 160°C to 165°C. The solution is titrated with a titrant (KOH concentration of 0.01 mol / L) in which 0.132 g of KOH is dissolved in 200 mL of benzyl alcohol, and the color change is yellow to red. It was calculated by taking it as the end point.
The unit of end group concentration is μequivalent/g.

<繊維>
ガラス繊維:日本電気硝子社製、ECS03T-296GH、平均繊維長3.0mm、短繊維直径10.0μm
<Fiber>
Glass fiber: ECS03T-296GH manufactured by Nippon Electric Glass Co., Ltd., average fiber length 3.0 mm, short fiber diameter 10.0 μm

<黒色着色剤>
カーボンブラック(三菱化学社製、MA600B)
<タルク>
ミクロンホワイト#5000S:林化成社製
<離型剤>
ライトアマイドWH255:共栄社化学社製
<Black colorant>
Carbon black (manufactured by Mitsubishi Chemical Corporation, MA600B)
<Talc>
Micron White #5000S: manufactured by Hayashi Kasei Co., Ltd. <Releasing agent>
Lightamide WH255: manufactured by Kyoeisha Chemical Co., Ltd.

実施例1
最終組成が、下記表1に示す組成となるように、半芳香族ポリアミド樹脂とタルクと離型剤と黒色着色剤をそれぞれ秤量し、ドライブレンドした後、二軸押出機(東芝機械社製、TEM26SS)のスクリュー根元から2軸スクリュー式カセットウェイングフィーダ(クボタ社製、CE-W-1-MP)を用いて投入した。黒色着色剤については、分量の範囲内の半芳香族ポリアミド樹脂の一部を用いてマスターバッチ化してから投入した。また、ガラス繊維については振動式カセットウェイングフィーダ(クボタ社製、CE-V-1B-MP)を用いて押出機のサイドから上述の二軸押出機に投入し、樹脂成分等と溶融混練し、ペレット(ポリアミド樹脂組成物)を得た。押出機の温度設定は、280℃とした。
Example 1
Semi-aromatic polyamide resin, talc, release agent and black colorant were weighed and dry-blended so that the final composition would be the composition shown in Table 1 below. TEM26SS) using a twin-screw cassette weighing feeder (CE-W-1-MP, manufactured by Kubota Corporation). As for the black colorant, a part of the semi-aromatic polyamide resin within the range of the amount was used to make a masterbatch and then added. In addition, the glass fiber is fed into the above-mentioned twin-screw extruder from the side of the extruder using a vibrating cassette weighing feeder (CE-V-1B-MP, manufactured by Kubota Corporation), and melted and kneaded with the resin component. , to obtain pellets (polyamide resin composition). The temperature setting of the extruder was 280°C.

<水分透過係数の測定>
上記で得られたペレットを用いて、日精樹脂工業社製、NEX80III-9Eを用い、シリンダー温度280℃、金型表面温度135℃で、100mm×100mm×1mm厚の試験片を射出成形した。
次に、図1に示すように、内径67mm、内部の高さ80mmのアルミ製の円筒状のカップ11の内部に25gの塩化カルシウム粒子12を入れた。カップの内部底面から50mmの位置において、上記試験片13を用いて封止し、40℃、相対湿度90%の雰囲気下に42時間静置した。塩化カルシウム粒子の質量を計測し、静置前との差分(増加分)を透過した水分量とし、水分透過係数を算出した。
水分透過係数の単位は、g・mm/day・m2である。
<Measurement of water permeability coefficient>
Using the pellets obtained above, using NEX80III-9E manufactured by Nissei Plastic Industry Co., Ltd., a test piece of 100 mm × 100 mm × 1 mm thickness was injection molded at a cylinder temperature of 280 ° C. and a mold surface temperature of 135 ° C.
Next, as shown in FIG. 1, 25 g of calcium chloride particles 12 were placed inside an aluminum cylindrical cup 11 having an inner diameter of 67 mm and an internal height of 80 mm. The test piece 13 was used to seal the cup at a position 50 mm from the inner bottom surface of the cup, and the cup was allowed to stand in an atmosphere of 40° C. and a relative humidity of 90% for 42 hours. The mass of the calcium chloride particles was measured, and the difference (increase) from before standing was taken as the amount of permeated water to calculate the water permeability coefficient.
The unit of moisture permeability coefficient is g·mm/day·m 2 .

Figure 0007194789000001
Figure 0007194789000001

<曲げ強度>
上記ペレットを120℃で4時間乾燥させた後、ファナック社製射出成形機(100T)を用いて、シリンダー温度280℃、金型の表面温度135℃の条件で、100mm×100mm×2mm厚の成形品を射出成形した。成形条件は、約0.5秒でキャビティの約95%を充填し、保圧をVP切り替え圧の約80%で10秒設定した。
得られた成形品の曲げ強度を、ISO-178基準に従って測定した。曲げ強度の単位は、MPaである。
<Bending strength>
After drying the pellets at 120°C for 4 hours, a 100mm x 100mm x 2mm thickness is molded using a Fanuc injection molding machine (100T) under the conditions of a cylinder temperature of 280°C and a mold surface temperature of 135°C. The product was injection molded. The molding conditions were about 95% filling of the cavity in about 0.5 seconds, and holding pressure was set at about 80% of the VP switching pressure for 10 seconds.
The flexural strength of the molded article obtained was measured according to the ISO-178 standard. The unit of bending strength is MPa.

実施例2
実施例1において、半芳香族ポリアミド樹脂をMP6-1に変更し、他は同様に行った。
Example 2
In Example 1, the semi-aromatic polyamide resin was changed to MP6-1, and the rest was carried out in the same manner.

比較例1
実施例1において、ガラス繊維を等量のガラスフレーク(日本板硝子社製ガラスフレークREF-015 平均厚さ5μm、平均粒径15μm)に変更し、他は同様に行った。
Comparative example 1
In Example 1, the glass fiber was changed to an equal amount of glass flakes (Glass flake REF-015 manufactured by Nippon Sheet Glass Co., Ltd., average thickness 5 μm, average particle size 15 μm), and other operations were performed in the same manner.

比較例2
実施例2において、半芳香族ポリアミド樹脂をMP6-2に変更し、他は同様に行った。
Comparative example 2
In Example 2, the semi-aromatic polyamide resin was changed to MP6-2, and the rest was carried out in the same manner.

Figure 0007194789000002
Figure 0007194789000002

上記結果から明らかなとおり、本発明の成形品は、機械的強度に優れた成形品が得られた。 As is clear from the above results, the molded article of the present invention was excellent in mechanical strength.

11 カップ
12 塩化カルシウム粒子
13 試験片
11 cup 12 calcium chloride particles 13 test piece

Claims (11)

半芳香族ポリアミド樹脂と、数平均繊維長が300μmを超える繊維を含み、前記半芳香族ポリアミド樹脂の末端カルボキシル基濃度が末端アミノ基濃度よりも高く、末端カルボキシル基濃度と末端アミノ基濃度の差が47μ当量/g以上100μ当量/g未満である、ポリアミド樹脂組成物から成形され、かつ、前記ポリアミド樹脂組成物は、1mmの厚さに成形し、40℃、相対湿度90%の条件下に42時間静置した後の水分透過係数が3.0g・mm/day・m2以下であり、前記繊維の数平均繊維長が1.0mm~6.0mmであり、カメラ部品である、成形品。 A semi-aromatic polyamide resin and a fiber having a number average fiber length exceeding 300 μm, wherein the terminal carboxyl group concentration of the semi-aromatic polyamide resin is higher than the terminal amino group concentration, and the difference between the terminal carboxyl group concentration and the terminal amino group concentration is 47 μ equivalent / g or more and less than 100 μ equivalent / g, and the polyamide resin composition is molded to a thickness of 1 mm, 40 ° C., under the conditions of 90% relative humidity A molded product having a moisture permeability coefficient of 3.0 g·mm/day·m 2 or less after being left to stand for 42 hours, a number average fiber length of 1.0 mm to 6.0 mm, and being a camera part. . 透明部材を有する車載カメラのカメラ部品の成形に用いる、請求項1に記載の成形品。 2. The molded article according to claim 1, which is used for molding a camera part of an on-vehicle camera having a transparent member. 前記繊維が炭素繊維およびガラス繊維から選択される少なくとも1種である、請求項1または2に記載の成形品。 The molded article according to claim 1 or 2, wherein said fiber is at least one selected from carbon fiber and glass fiber. 前記繊維が、表面処理剤および集束剤の少なくとも一方で処理されている、請求項1~3のいずれか1項に記載の成形品。 The molded article according to any one of claims 1 to 3, wherein the fibers are treated with at least one of a surface treatment agent and a sizing agent. さらに、黒色着色剤を含む、請求項1~4のいずれか1項に記載の成形品。 The molded article according to any one of claims 1 to 4, further comprising a black colorant. さらに、タルクを含む、請求項1~5のいずれか1項に記載の成形品。 The molded article according to any one of claims 1 to 5, further comprising talc. さらに、黒色着色剤とタルクを含み、前記成形品における、黒色着色剤とタルクの質量比(黒色着色剤/タルク)が1.5~2.5である、請求項1~6のいずれか1項に記載の成形品。 Any one of claims 1 to 6, further comprising a black coloring agent and talc, wherein the mass ratio of the black coloring agent to talc (black coloring agent/talc) in the molded product is 1.5 to 2.5. Articles described in paragraph. 射出成形品である、請求項1~7のいずれか1項に記載の成形品。 The molded article according to any one of claims 1 to 7, which is an injection molded article. 前記カメラ部品の最大長さが、15~40mmである、請求項1~8のいずれか1項に記載の成形品。 The molded article according to any one of claims 1 to 8, wherein the camera part has a maximum length of 15 to 40 mm. 前記カメラ部品が、前記ポリアミド樹脂組成物に由来する部材を含み、前記部材の割合が、1~99質量%である、請求項1~9のいずれか1項に記載の成形品。 The molded article according to any one of claims 1 to 9, wherein the camera part contains a member derived from the polyamide resin composition, and the proportion of the member is 1 to 99% by mass. 半芳香族ポリアミド樹脂と、数平均繊維長が300μmを超える繊維を含み、前記半芳香族ポリアミド樹脂の末端カルボキシル基濃度が末端アミノ基濃度よりも高い、ポリアミド樹脂組成物を射出成形することを含む、請求項1~10のいずれか1項に記載のカメラ部品である成形品の製造方法。 Injection molding a polyamide resin composition comprising a semi-aromatic polyamide resin and fibers having a number average fiber length exceeding 300 μm, wherein the concentration of terminal carboxyl groups of the semi-aromatic polyamide resin is higher than the concentration of terminal amino groups. 11. A method for manufacturing a molded product which is a camera part according to any one of claims 1 to 10.
JP2021126669A 2016-10-07 2021-08-02 Articles and methods of manufacturing articles Active JP7194789B2 (en)