JP7067542B2 - Decorative molded products and their manufacturing methods - Google Patents

Decorative molded products and their manufacturing methods Download PDF

Info

Publication number
JP7067542B2
JP7067542B2 JP2019201122A JP2019201122A JP7067542B2 JP 7067542 B2 JP7067542 B2 JP 7067542B2 JP 2019201122 A JP2019201122 A JP 2019201122A JP 2019201122 A JP2019201122 A JP 2019201122A JP 7067542 B2 JP7067542 B2 JP 7067542B2
Authority
JP
Japan
Prior art keywords
molded product
gloss
resin
layer
pattern layer
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
JP2019201122A
Other languages
Japanese (ja)
Other versions
JP2020040406A (en
Inventor
健太 高山
孝志 飯塚
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Dai Nippon Printing Co Ltd
Original Assignee
Dai Nippon Printing Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Dai Nippon Printing Co Ltd filed Critical Dai Nippon Printing Co Ltd
Priority to JP2019201122A priority Critical patent/JP7067542B2/en
Publication of JP2020040406A publication Critical patent/JP2020040406A/en
Application granted granted Critical
Publication of JP7067542B2 publication Critical patent/JP7067542B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Description

本発明は、加飾成形品及びその製造方法に関する。 The present invention relates to a decorative molded product and a method for producing the same.

建材、自動車内装品、家電製品、OA機器などには表面に木目調や金属調などの装飾が施された成形品が利用されている。これらの成形品は複雑な三次元形状を有するものが多く、従来、その複雑な形状からなる成形品に意匠性の高い装飾を簡便に施す方法が検討されている。 Molded products with wood grain or metallic decoration on the surface are used for building materials, automobile interior products, home appliances, OA equipment, and the like. Many of these molded products have a complicated three-dimensional shape, and conventionally, a method of easily applying a highly-designed decoration to a molded product having the complicated shape has been studied.

こうした装飾方法の一つとして、水圧を利用した水圧転写法が知られている。水圧転写法では、水溶性または水膨潤性の水溶性フィルムに、所望の装飾層を印刷した転写フィルムを用意し、該転写フィルムの装飾層に、有機溶剤からなる活性剤組成物を塗布して、該装飾層を膨潤、粘着化させる(これを活性化という)。その前または後に、上記転写フィルムを転写用の装飾層(印刷層)面を上面にして、水面上に浮遊させ、次いで、該転写フィルム上に被転写体となる物品を押圧して、水圧によって転写フィルムを被転写体の装飾処理をすべき被転写面に密着させた後、水溶性フィルムを除去して装飾層を転写する。 As one of such decoration methods, a hydraulic transfer method using hydraulic pressure is known. In the hydraulic transfer method, a transfer film having a desired decorative layer printed on a water-soluble or water-swellable water-soluble film is prepared, and an activator composition composed of an organic solvent is applied to the decorative layer of the transfer film. , The decorative layer is swollen and adhered (this is called activation). Before or after that, the transfer film is suspended on the water surface with the decorative layer (printing layer) surface for transfer as the upper surface, and then the article to be transferred is pressed onto the transfer film by water pressure. After the transfer film is brought into close contact with the surface to be transferred to be decorated, the water-soluble film is removed and the decorative layer is transferred.

このような水圧転写法は、立体面への転写加工性、クリア塗装官等の「深み」や、高品質な柄表現が出来るなどの意匠性の点で、優れた曲面加飾法であることが知られている。このような水圧転写法を用いて得られた加飾成形品は、樹脂成形品に対して高い立体感を表出した意匠を有することが知られている。 Such a hydraulic transfer method is an excellent curved surface decoration method in terms of transfer processability to a three-dimensional surface, "depth" of a clear painter, etc., and designability such as high-quality pattern expression. It has been known. It is known that the decorative molded product obtained by using such a hydraulic transfer method has a design that expresses a high three-dimensional effect with respect to the resin molded product.

例えば、特許文献1には、水溶性フィルム上に意匠層を有する水圧転写フィルムを用いて、バインダー樹脂及び艶消し剤を含む低艶部分と、アクリルポリマーポリオールまたはその硬化物を含む高艶部分との艶の差によって強いコントラストを表現する手法により、凹凸感を有する意匠を表現する加飾成形品を製造できることが開示されている。 For example, in Patent Document 1, a hydraulic transfer film having a design layer on a water-soluble film is used to provide a low-gloss portion containing a binder resin and a matting agent, and a high-gloss portion containing an acrylic polymer polyol or a cured product thereof. It is disclosed that a decorative molded product that expresses a design having a feeling of unevenness can be manufactured by a method of expressing a strong contrast by a difference in gloss.

特開2013-240976号公報Japanese Unexamined Patent Publication No. 2013-240976

しかしながら、例えば特許文献1に開示されたような方法では、高艶部分であるアクリルポリマーポリオール層の転写加工性がやや劣る。また、この方法においては、低艶部分と高艶部分の2層を設ける必要がある。よって、特許文献1に開示された方法によって、加飾成形品に高い立体感を表出させるためには、生産コストが増大するという問題がある。
このような状況下、本発明は、高い立体感を表出する意匠を有し、かつ、生産コストが低減された加飾成形品、及びその製造方法を提供することを主な目的とする。
However, for example, in the method disclosed in Patent Document 1, the transfer processability of the acrylic polymer polyol layer, which is a high-gloss portion, is slightly inferior. Further, in this method, it is necessary to provide two layers, a low gloss portion and a high gloss portion. Therefore, there is a problem that the production cost increases in order to express a high three-dimensional effect in the decorative molded product by the method disclosed in Patent Document 1.
Under such circumstances, it is a main object of the present invention to provide a decorative molded product having a design that expresses a high three-dimensional effect and having a reduced production cost, and a method for producing the same.

本発明者らは、上記課題を解決するために鋭意研究を重ねた。その結果、高艶調成形品と、当該高艶調成形品表面の一部に設けられた絵柄層とを有する加飾成形品は、高い立体感と、観察する角度によって意匠性が変化するような独特の意匠を有する加飾成形品とすることができ、さらに、加飾成形品の生産コストを低減できることを見出した。本発明は、かかる知見に基づいて、更に検討を重ねることにより完成したものである。 The present inventors have conducted extensive research to solve the above problems. As a result, the decorative molded product having the high-gloss-like molded product and the pattern layer provided on a part of the surface of the high-gloss-like molded product has a high three-dimensional effect and the design property changes depending on the observation angle. It has been found that a decorative molded product having a unique design can be obtained, and further, the production cost of the decorative molded product can be reduced. The present invention has been completed by further studies based on such findings.

即ち、本発明は、下記に掲げる態様の発明を提供する。
項1. 高艶調成形品と、前記高艶調成形品表面の一部に設けられた絵柄層とを有する、加飾成形品。
項2. 前記高艶調成形品は、前記絵柄層側の表面のグロス値(60°)が70以上である、項1に記載の加飾成形品。
項3. 前記高艶調成形品は、基材層と、高艶樹脂層との積層体であり、
前記高艶樹脂層が前記絵柄層側に積層されている、項1または2に記載の加飾成形品。
項4. 前記高艶樹脂層は、アクリルポリマーポリオールを含む樹脂組成物の硬化物により形成されている、項3に記載の加飾成形品。
項5. 前記絵柄層は、水圧転写法により形成された、項1~4のいずれかに記載の加飾成形品。
項6. 前記絵柄層上にトップコート層をさらに有する、項1~5のいずれかに記載の加飾成形品。
項7. 前記トップコート層は、艶消し調である、項6に記載の加飾成形品。
項8. 高艶調成形品と、前記高艶調成形品表面の一部に設けられた絵柄層とを有する、加飾成形品の製造方法であって、
水溶性フィルムと、前記水溶性フィルム上の一部に設けられた絵柄層とを有する水圧転写フィルムを用いて、高艶調成形品上に絵柄層を転写する工程を備える、加飾成形品の製造方法。
項9. 前記高艶調成形品は、表面のグロス値(60°)が70以上である、項8に記載の加飾成形品の製造方法。
項10. 前記高艶調成形品は、基材層と、高艶樹脂層との積層体であり、
前記高艶樹脂層が前記絵柄層側に積層されている、項8または9に記載の加飾成形品の製造方法。
That is, the present invention provides the inventions of the following aspects.
Item 1. A decorative molded product having a high-gloss-like molded product and a pattern layer provided on a part of the surface of the high-gloss-like molded product.
Item 2. Item 2. The decorative molded product according to Item 1, wherein the high-gloss molded product has a gloss value (60 °) of the surface on the pattern layer side of 70 or more.
Item 3. The high-gloss molded product is a laminate of a base material layer and a high-gloss resin layer.
Item 2. The decorative molded product according to Item 1 or 2, wherein the high-gloss resin layer is laminated on the pattern layer side.
Item 4. Item 3. The decorative molded product according to Item 3, wherein the high-gloss resin layer is formed of a cured product of a resin composition containing an acrylic polymer polyol.
Item 5. Item 2. The decorative molded product according to any one of Items 1 to 4, wherein the pattern layer is formed by a hydraulic transfer method.
Item 6. Item 2. The decorative molded product according to any one of Items 1 to 5, further comprising a top coat layer on the pattern layer.
Item 7. Item 6. The decorative molded product according to Item 6, wherein the top coat layer has a matte tone.
Item 8. A method for manufacturing a decorative molded product, which comprises a high-gloss molded product and a pattern layer provided on a part of the surface of the high-gloss molded product.
A decorative molded product comprising a step of transferring a pattern layer onto a high-gloss-like molded product using a hydraulic transfer film having a water-soluble film and a pattern layer provided on a part of the water-soluble film. Production method.
Item 9. Item 8. The method for manufacturing a decorative molded product according to Item 8, wherein the high-gloss molded product has a surface gloss value (60 °) of 70 or more.
Item 10. The high-gloss molded product is a laminate of a base material layer and a high-gloss resin layer.
Item 8. The method for manufacturing a decorative molded product according to Item 8 or 9, wherein the high-gloss resin layer is laminated on the pattern layer side.

本発明によれば、高い立体感と、観察する角度によって意匠性が変化するような独特の意匠を有しており、さらには、転写加工性の低い意匠層を設ける必要が無いため、生産コストを低減することもできる加飾成形品を提供することができる。さらに、本発明によれば、当該加飾成形品の好適な製造方法を提供することもできる。 According to the present invention, it has a high three-dimensional effect and a unique design in which the design property changes depending on the observation angle, and further, it is not necessary to provide a design layer having low transfer processability, so that the production cost is high. It is possible to provide a decorative molded product that can also reduce the amount of. Further, according to the present invention, it is also possible to provide a suitable manufacturing method for the decorative molded product.

本発明の加飾成形品の構成の一例を示す概略断面図である。It is a schematic sectional drawing which shows an example of the structure of the decorative molded article of this invention. 本発明の加飾成形品の構成の一例を示す概略断面図である。It is a schematic sectional drawing which shows an example of the structure of the decorative molded article of this invention. 本発明の加飾成形品の構成の一例を示す概略断面図である。It is a schematic sectional drawing which shows an example of the structure of the decorative molded article of this invention. 本発明の加飾成形品の製造に用いる水圧転写フィルムの構成の一例を示す概略断面図である。It is a schematic sectional drawing which shows an example of the structure of the hydraulic transfer film used for manufacturing the decorative molded article of this invention.

本発明の加飾成形品は、高艶調成形品と、前記高艶調成形品表面の一部に設けられた絵柄層とを有することを特徴とする。本発明加飾成形品においては、このような構成を備えているため、高い立体感と、観察する角度によって意匠性が変化するような独特の意匠を有しており、さらには、転写加工性の低い意匠層を設ける必要が無いため、生産コストを低減することもできる。本発明の加飾成形品は、後述の水圧転写法によって好適に製造することができる。なお、本発明において、「高艶調成形品表面の一部に設けられた絵柄層」には、高艶調成形品の全面に、絵柄層が設けられた部分と設けられていない部分とがパターン状または非パターン状に形成されている態様が含まれる。 The decorative molded product of the present invention is characterized by having a high-gloss-like molded product and a pattern layer provided on a part of the surface of the high-gloss-like molded product. Since the decorative molded product of the present invention has such a configuration, it has a high three-dimensional effect, a unique design in which the design changes depending on the observation angle, and further, transfer processability. Since it is not necessary to provide a low design layer, the production cost can be reduced. The decorative molded product of the present invention can be suitably produced by the hydraulic transfer method described later. In the present invention, the "pattern layer provided on a part of the surface of the high-gloss-like molded product" includes a portion provided with the pattern layer and a portion not provided on the entire surface of the high-gloss-like molded product. Aspects formed in a patterned or non-patterned manner are included.

前述の通り、従来の加飾成形品(特に、水圧転写法によって製造される加飾成形品)においては、成形品上に、絵柄層と、低艶部分と高艶部分とを有する意匠層とを形成することにより、高い立体感を表出した意匠が付与されている。そのような意匠は、例えば、水溶性フィルム上に、上記低艶部分と高艶部分とを有する意匠層と、上記絵柄層とを順に有する水圧転写フィルムを用いた水圧転写法により形成される。しかしながら、このような水圧転写フィルムによる加飾は、意匠層においてアクリルポリマーポリオールが使用されるため、転写加工性が十分ではない。さらに、この方法においては、低艶部分と高艶部分の2層を設ける必要がある。このため、従来の方法によって、加飾成形品に高い立体感を表出させるためには、生産コストが増大するという問題がある。 As described above, in the conventional decorative molded product (particularly, the decorative molded product manufactured by the hydraulic transfer method), a pattern layer and a design layer having a low-gloss portion and a high-gloss portion are provided on the molded product. By forming the above, a design that expresses a high three-dimensional effect is given. Such a design is formed, for example, by a hydraulic transfer method using a hydraulic transfer film having the low-gloss portion and the high-gloss portion in order on a water-soluble film. However, such decoration with a hydraulic transfer film does not have sufficient transfer processability because an acrylic polymer polyol is used in the design layer. Further, in this method, it is necessary to provide two layers, a low gloss portion and a high gloss portion. Therefore, there is a problem that the production cost increases in order to give a high three-dimensional effect to the decorative molded product by the conventional method.

これに対して、本発明の加飾成形品においては、加飾前の成形品の表面を、高艶調(すなわち、成形品表面自体を高艶調とする)とし、その高艶調成形品の表面の一部に絵柄層2を設けることにより、高い立体感と、観察する角度によって意匠性が変化するような独特の意匠を有しており、かつ、転写加工性の低い意匠層を設ける必要が無いため、生産コストを低減することもできる。以下、本発明の加飾成形品について、図1~3を参照しながら詳述する。 On the other hand, in the decorative molded product of the present invention, the surface of the molded product before decoration has a high gloss tone (that is, the surface of the molded product itself has a high gloss tone), and the surface of the molded product has a high gloss tone. By providing the pattern layer 2 on a part of the surface of the above, a design layer having a high three-dimensional effect and a unique design in which the design property changes depending on the observation angle is provided, and the transfer processability is low. Since there is no need, the production cost can be reduced. Hereinafter, the decorative molded product of the present invention will be described in detail with reference to FIGS. 1 to 3.

[加飾成形品]
図1~3は、本発明の加飾成形品の構成の一例を示す概略断面図である。図1に示されるように、本発明の加飾成形品10は、高艶調成形品1及び絵柄層2を有する。高艶調成形品1は、少なくとも絵柄層2側の表面が高艶調である。
[Decorative molded products]
1 to 3 are schematic cross-sectional views showing an example of the configuration of the decorative molded product of the present invention. As shown in FIG. 1, the decorative molded product 10 of the present invention has a high-gloss-like molded product 1 and a pattern layer 2. In the high-gloss molded product 1, at least the surface on the pattern layer 2 side has a high-gloss tone.

絵柄層2は、高艶調成形品1の高艶調表面の一部に設けられている。すなわち、高艶調成形品1の表面は、絵柄層2が設けられた部分と、絵柄層2が設けられていない部分とからなる。このため、本発明の加飾成形品10を絵柄層2側から見た場合、絵柄層2が設けられた部分と、絵柄層2が設けられていない、高艶調成形品1の高艶調表面とが視認される。本発明の加飾成形品10は、このような構成を備えるため、絵柄層2と絵柄層2が設けられていない高艶調成形品1の高艶調表面の艶のコントラストにより、高い立体感と、観察する角度によって意匠性が変化するような独特の意匠を有する。 The pattern layer 2 is provided on a part of the high-gloss-like surface of the high-gloss-like molded product 1. That is, the surface of the high-gloss molded product 1 is composed of a portion provided with the pattern layer 2 and a portion not provided with the pattern layer 2. Therefore, when the decorative molded product 10 of the present invention is viewed from the pattern layer 2 side, the portion provided with the pattern layer 2 and the high gloss tone of the high gloss tone molded product 1 without the pattern layer 2 are provided. The surface is visible. Since the decorative molded product 10 of the present invention has such a configuration, the high-gloss-like molded product 1 without the pattern layer 2 and the pattern layer 2 has a high three-dimensional effect due to the gloss contrast of the high-gloss-like surface. And, it has a unique design whose design changes depending on the observation angle.

また、図2に示されるように、本発明の加飾成形品10において、高艶調成形品1は、基材層1aと、高艶樹脂層1bとの積層体であり、当該高艶樹脂層1bが絵柄層2側に積層されたものであってもよい。 Further, as shown in FIG. 2, in the decorative molded product 10 of the present invention, the high-gloss-like molded product 1 is a laminate of the base material layer 1a and the high-gloss resin layer 1b, and the high-gloss resin. The layer 1b may be laminated on the pattern layer 2 side.

さらに、図3に示されるように、本発明の加飾成形品10は、必要に応じて、絵柄層2上にトップコート層3をさらに有していてもよい。以下、本発明の加飾成形品10を構成する各層について詳述する。 Further, as shown in FIG. 3, the decorative molded product 10 of the present invention may further have a top coat layer 3 on the pattern layer 2, if necessary. Hereinafter, each layer constituting the decorative molded product 10 of the present invention will be described in detail.

<高艶調成形品1>
高艶調成形品1は、少なくとも絵柄層2側の表面が、高艶調である。前述の通り、本発明の加飾成形品10においては、高艶調成形品1の高艶調表面の一部が、絵柄層2によって覆われているため、加飾成形品10を絵柄層2側から見た場合に、絵柄層2と絵柄層2が設けられていない高艶調成形品1の高艶調表面の艶のコントラストにより、高い立体感と、観察する角度によって意匠性が変化するような独特の意匠を表出する。
<High gloss molded product 1>
In the high-gloss molded product 1, at least the surface on the pattern layer 2 side has a high-gloss tone. As described above, in the decorative molded product 10 of the present invention, since a part of the high-gloss-like surface of the high-gloss-like molded product 1 is covered with the pattern layer 2, the decorative molded product 10 is referred to as the pattern layer 2. When viewed from the side, the contrast between the high-gloss tone surface of the high-gloss tone molded product 1 without the pattern layer 2 and the high-gloss tone surface of the pattern layer 2 changes the high three-dimensional appearance and the design depending on the observation angle. It expresses such a unique design.

本発明の加飾成形品10が奏する意匠性をより一層高める観点からは、高艶調成形品1の絵柄層2側の表面のグロス値(60°)としては、好ましくは70以上、より好ましくは90以上が挙げられる。なお、グロス値(60°)の上限値としては、95程度が好ましい。当該本発明において、当該グロス値(60°)は、市販のグロスメーターを用いて、艶消調成形品の表面に対する光の入射角60°の条件として測定されたグロス値であり、任意の3点を測定した平均値である。 From the viewpoint of further enhancing the designability of the decorative molded product 10 of the present invention, the gloss value (60 °) of the surface of the high-gloss molded product 1 on the pattern layer 2 side is preferably 70 or more, more preferably 70 or more. 90 or more can be mentioned. The upper limit of the gloss value (60 °) is preferably about 95. In the present invention, the gloss value (60 °) is a gloss value measured using a commercially available gloss meter under the condition of an incident angle of light of 60 ° to the surface of the matte-adjusted molded product, and is any 3 It is the average value of measured points.

高艶調成形品1の表面を高艶調にする方法としては、特に制限されないが、基材層1aと高艶樹脂層1bとの積層体とすること好ましい。当該積層体からなる高艶調成形品1において、高艶樹脂層1bを絵柄層1a側に積層することにより、高艶調成形品1の表面を高艶調にすることができる。 The method for making the surface of the high-gloss molded product 1 high-gloss is not particularly limited, but a laminate of the base material layer 1a and the high-gloss resin layer 1b is preferable. In the high-gloss-like molded product 1 made of the laminated body, the surface of the high-gloss-like molded product 1 can be made high-gloss by laminating the high-gloss resin layer 1b on the pattern layer 1a side.

高艶樹脂層1bを構成する素材としては、高艶調成形品1の表面を高艶調にできる素材であれば、特に制限されないが、本発明の加飾成形品10が奏する意匠性をより一層高める観点からは、好ましくはアクリルポリマーポリオールを含む樹脂組成物の硬化物が挙げられる。当該硬化物は完全硬化されたものであってもよいし、半硬化状態であってもよい。また、アクリルポリマーポリオールを含む樹脂組成物と該樹脂組成物の硬化物が混合された状態であってもよい。また、高艶調成形品1を形成する樹脂組成物には、アクリルポリマーポリオールに加えて、さらにイソシアネートを含有させることもできる。イソシアネートはアクリルポリマーポリオールの硬化剤であって、イソシアネートを含有させることで、当該樹脂組成物の少なくとも一部を硬化状態又は半硬化状態とする。 The material constituting the high-gloss resin layer 1b is not particularly limited as long as it is a material capable of making the surface of the high-gloss-like molded product 1 high-gloss, but the designability of the decorative molded product 10 of the present invention is further improved. From the viewpoint of further enhancing, a cured product of a resin composition containing an acrylic polymer polyol is preferable. The cured product may be completely cured or may be in a semi-cured state. Further, the resin composition containing the acrylic polymer polyol and the cured product of the resin composition may be in a mixed state. Further, the resin composition forming the high-gloss molded product 1 may further contain isocyanate in addition to the acrylic polymer polyol. Isocyanate is a curing agent for an acrylic polymer polyol, and by containing isocyanate, at least a part of the resin composition is put into a cured state or a semi-cured state.

(アクリルポリマーポリオール)
上記アクリルポリマーポリオールは、ゲルパーミエーションクロマトグラフィー(GPC)法により求められる、標準ポリスチレンで換算された重量平均分子量が1,000~100,000であることが好ましく、5,000~80,000であることがより好ましく、20,000~50,000であることが特に好ましい。
(Acrylic polymer polyol)
The acrylic polymer polyol preferably has a weight average molecular weight of 1,000 to 100,000 converted to standard polystyrene, which is determined by a gel permeation chromatography (GPC) method, and is preferably 5,000 to 80,000. It is more preferably 20,000 to 50,000, and particularly preferably 20,000 to 50,000.

また、アクリルポリマーポリオールとしては、水酸基価が30~130mgKOH/gのものが好ましく、50~130mgKOH/gのものがより好ましく、60~120mgKOH/gのものがさらに好ましい。 The acrylic polymer polyol preferably has a hydroxyl value of 30 to 130 mgKOH / g, more preferably 50 to 130 mgKOH / g, and even more preferably 60 to 120 mgKOH / g.

(イソシアネート)
イソシアネートとしては、分子中に2個以上のイソシアネート基を有する多価イソシアネートであればよく、例えば、2,4-トリレンジイソシアネート(TDI)、キシレンジイソシアネート(XDI)、ナフタレンジイソシアネート、4,4′-ジフェニルメタンジイソシアネートなどの芳香族イソシアネート、或いは、1,6-ヘキサメチレンジイソシアネート(HMDI)、イソホロンジイソシアネート(IPDI)、メチレンジイソシアネート(MDI)、水素添加トリレンジイソシアネート、水素添加ジフェニルメタンジイソシアネートなどの脂肪族(乃至は脂環式)イソシアネートなどのポリイソシアネートが用いられる。
(Isocyanate)
The isocyanate may be a polyvalent isocyanate having two or more isocyanate groups in the molecule, for example, 2,4-tolylene diisocyanate (TDI), xylene diisocyanate (XDI), naphthalene diisocyanate, 4,4'-. Aromatic isocyanates such as diphenylmethane diisocyanate, or aliphatics (or or) such as 1,6-hexamethylene diisocyanate (HMDI), isophorone diisocyanate (IPDI), methylene diisocyanate (MDI), hydrogenated tolylene diisocyanate, and hydrogenated diphenylmethane diisocyanate. Polyisocyanate such as alicyclic) isocyanate is used.

また、必要に応じて、イソシアネート基を適当なブロック剤により保護して不活性化し、加熱によりイソシアネート基が再生するブロックイソシアネートを使用してもよい。ブロック剤としては、例えばフェノール、アルコール、マロン酸ジメチル、アセト酢酸エチル等の活性メチレン、オキシム等、公知のブロック剤を用いてもよい。 Further, if necessary, blocked isocyanate may be used in which the isocyanate group is protected with an appropriate blocking agent and inactivated, and the isocyanate group is regenerated by heating. As the blocking agent, known blocking agents such as phenol, alcohol, active methylene such as dimethyl malonate and ethyl acetoacetate, and oxime may be used.

ブロックイソシアネートを使用することにより、高艶樹脂層1bにより高い成形性を付与することができ、所望形状に成形した後に成形品を加熱処理し、イソシアネート基を再生、ポリオールと反応、硬化することにより、絵柄層2と良好な密着性を発現できる。 By using blocked isocyanate, high glossability can be imparted to the high-gloss resin layer 1b, and after molding into a desired shape, the molded product is heat-treated to regenerate the isocyanate group, react with the polyol, and cure. , Good adhesion to the pattern layer 2 can be exhibited.

上記高艶樹脂層1bを構成する樹脂組成物には、ウレタン樹脂、(メタ)アクリル樹脂、(メタ)アクリル・ウレタン共重合体樹脂、塩化ビニル-酢酸ビニル共重合体、ポリエステル樹脂、ブチラール樹脂、塩素化ポリプロピレン、塩素化ポリエチレンなどを含有させてもよい。これらのうち、特にウレタン樹脂はアクリルポリマーポリオールとの相溶性が高く、好ましい。 The resin composition constituting the high gloss resin layer 1b includes urethane resin, (meth) acrylic resin, (meth) acrylic / urethane copolymer resin, vinyl chloride-vinyl acetate copolymer, polyester resin, butyral resin, and the like. It may contain chlorinated polypropylene, chlorinated polyethylene and the like. Of these, urethane resin is particularly preferable because it has high compatibility with acrylic polymer polyol.

また、上記高艶樹脂層1bには、本発明の効果を阻害しない範囲内で着色剤を添加してもよい。着色剤としては、後述する絵柄層で用いられるものと同様のものを用いることができる。 Further, a colorant may be added to the high gloss resin layer 1b as long as the effect of the present invention is not impaired. As the colorant, the same colorant as that used in the pattern layer described later can be used.

(ウレタン樹脂)
ウレタン樹脂としては、非架橋型のもの、すなわち、3次元架橋して網目状の立体的分子構造を持ったものではなく、線状の分子構造を持った熱可塑性樹脂となったものを選択することが好ましい。このような非架橋型のウレタン樹脂としては、ポリオール成分として、ポリエステルポリオール、ポリエーテルポリオール、ポリカーボネートポリオール、ポリカプロラクトンポリオール、ポリエチレングリコール、ポリプロピレングリコール等のポリオールを主剤とし、イソシアネートと反応させてなる非架橋型ウレタン樹脂を使用でき、成形性、耐熱性、耐候性、絵柄層2との密着性等の観点から、ポリエステルポリオールと、ヘキサメチレンジイソシアネート等のイソシアネートとの組合せにより合成されるものが特に好ましい。通常ポリオール1分子中の水酸基数及びイソシアネート1分子中のイソシアネート基はそれぞれ平均2である。
(Urethane resin)
As the urethane resin, a non-crosslinked type, that is, a thermoplastic resin having a linear molecular structure rather than a three-dimensionally crosslinked one having a network-like three-dimensional molecular structure is selected. Is preferable. As such a non-crosslinked urethane resin, a polyester polyol, a polyether polyol, a polycarbonate polyol, a polycaprolactone polyol, a polyethylene glycol, a polypropylene glycol or the like is used as a main component as a polyol component, and the non-crosslinked urethane resin is reacted with isocyanate. A type urethane resin can be used, and one synthesized by a combination of a polyester polyol and an isocyanate such as hexamethylene diisocyanate is particularly preferable from the viewpoints of moldability, heat resistance, weather resistance, adhesion to the pattern layer 2, and the like. Normally, the number of hydroxyl groups in one molecule of polyol and the number of isocyanate groups in one molecule of isocyanate are 2 on average.

また、ウレタン樹脂としては、ポリオール成分、ポリアミン成分及びイソシアネートの組合せより合成されるウレタンウレア樹脂が好ましく用いられ、ポリオール成分やイソシアネートとしては、前述したものを用いることができる。 Further, as the urethane resin, a urethane urea resin synthesized from a combination of a polyol component, a polyamine component and an isocyanate is preferably used, and as the polyol component and an isocyanate, the above-mentioned ones can be used.

ウレタン樹脂としては、ガラス転移点が100℃以下のものが好ましく、20~100℃のものがより好ましい。ウレタン樹脂のガラス転移点が100℃以下であると、高艶部分2bの常温における柔軟性に優れ、20℃以上であると、加熱により凝集力が著しく低下したり、高艶樹脂層1bが水圧転写時に水に溶解することがなく、好ましい。 The urethane resin preferably has a glass transition point of 100 ° C. or lower, and more preferably 20 to 100 ° C. When the glass transition point of the urethane resin is 100 ° C. or lower, the flexibility of the high-glossy portion 2b at room temperature is excellent, and when it is 20 ° C. or higher, the cohesive force is significantly reduced by heating, or the high-gloss resin layer 1b has a water pressure. It is preferable because it does not dissolve in water during transfer.

高艶樹脂層1bを構成する樹脂組成物におけるアクリルポリマーポリオール又はアクリルポリマーポリオールに必要に応じて添加されるイソシアネートの合計量とウレタン樹脂との比率は、通常質量比で99:1~50:50であり、95:5~50:50であることが好ましく、90:10~60:40であるとより好ましく、80:20~68:32であることが特に好ましい。 The ratio of the total amount of isocyanate added to the acrylic polymer polyol or the acrylic polymer polyol as needed in the resin composition constituting the high gloss resin layer 1b to the urethane resin is usually 99: 1 to 50:50 in terms of mass ratio. It is preferably 95: 5 to 50:50, more preferably 90:10 to 60:40, and particularly preferably 80:20 to 68:32.

高艶樹脂層1bは、高艶樹脂層1bを構成する樹脂組成物(例えば、前述のアクリルポリマーポリオール、イソシアネート、ウレタン樹脂、及びその他の樹脂)を溶媒に溶解した塗工液を、公知の方法で塗布し、必要に応じて乾燥し、硬化して形成することができる。高艶樹脂層1bの厚みについては、好ましくは1~25μm程度であり、より好ましくは、1~15の範囲である。 The high-gloss resin layer 1b is a known method using a coating liquid in which a resin composition (for example, the above-mentioned acrylic polymer polyol, isocyanate, urethane resin, and other resins) constituting the high-gloss resin layer 1b is dissolved in a solvent. It can be applied with, dried if necessary, and cured to form. The thickness of the high-gloss resin layer 1b is preferably about 1 to 25 μm, and more preferably in the range of 1 to 15.

基材層1aを構成する素材としては、例えば、ポリスチレン樹脂、アクリロニトリル-ブタジエン-スチレン共重合体(ABS樹脂)、ポリカーボネート樹脂、メラミン樹脂、フェノール樹脂、尿素樹脂、繊維系樹脂、ポリエチレン、ポリプロピレンなどの樹脂、あるいはこれらを混合した樹脂のほか、鉄、アルミニウム、銅などの金属、陶磁器、ガラス、琺瑯などのセラミックス、木材などの材料からなる構造体を使用することができる。また、基材層1aの形状についても、特に制限されず、平面形状である二次元形状であってもよいし、凹凸形状や曲面形状などの三次元形状であってもよい。高艶調成形品1としては、樹脂製構造体が多用される。 Examples of the material constituting the base material layer 1a include polystyrene resin, acrylonitrile-butadiene-styrene copolymer (ABS resin), polycarbonate resin, melamine resin, phenol resin, urea resin, fiber resin, polyethylene, polypropylene and the like. In addition to resins or resins in which these are mixed, structures made of metals such as iron, aluminum and copper, ceramics such as ceramics, glass and amber, and materials such as wood can be used. Further, the shape of the base material layer 1a is not particularly limited, and may be a two-dimensional shape that is a planar shape, or a three-dimensional shape such as an uneven shape or a curved surface shape. As the high-gloss molded product 1, a resin structure is often used.

また、本発明においては、高艶調成形品1を、前述の高艶樹脂層1aと同様にして、アクリルポリマーポリオールを含む樹脂組成物の硬化物により形成してもよい。この場合、高艶調成形品1の形状については、特に制限されず、平面形状である二次元形状であってもよいし、凹凸形状や曲面形状などの三次元形状であってもよい。高艶調成形品1としては、樹脂製構造体が多用される。高艶調成形品1は、例えば前述のような素材を用いて、公知の成形方法で作製することができる。 Further, in the present invention, the high-gloss molded product 1 may be formed from a cured product of a resin composition containing an acrylic polymer polyol in the same manner as the above-mentioned high-gloss resin layer 1a. In this case, the shape of the high-gloss-like molded product 1 is not particularly limited, and may be a two-dimensional shape that is a planar shape, or a three-dimensional shape such as an uneven shape or a curved surface shape. As the high-gloss molded product 1, a resin structure is often used. The high-gloss molded product 1 can be manufactured by a known molding method using, for example, the above-mentioned materials.

<絵柄層2>
絵柄層2は、加飾成形品10に装飾性を与える層である。絵柄層2によって形成される模様は、特に限定されず、例えば、木目模様、大理石模様、大理石模様(例えばトラバーチン大理石模様)等の岩石の表面を模した石目模様、布目や布状の模様を模した布地模様、タイル貼模様、煉瓦積模様など挙げられ、これらを複合した寄木、パッチワーク等の模様も挙げられる。
<Picture layer 2>
The pattern layer 2 is a layer that imparts decorativeness to the decorative molded product 10. The pattern formed by the pattern layer 2 is not particularly limited, and for example, a stone pattern imitating the surface of rock such as a wood grain pattern, a marble pattern, and a marble pattern (for example, a travertin marble pattern), a cloth pattern, or a cloth-like pattern can be used. Examples include imitated fabric patterns, tiled patterns, and brickwork patterns, as well as patterns such as parquet and patchwork that combine these patterns.

本発明の加飾成形品10において、絵柄層2は、高艶調成形品1表面の一部に設けられ、絵柄層2が設けられていない抜けの部分を有している。例えば、木目模様においては、導管部分が絵柄の抜けになり、それ以外の部分に絵柄が設けられる。このような絵柄層の構成により、本発明の加飾成形品10は、絵柄層2が設けられていない抜けの部分である高艶調成形品1の高艶調表面と絵柄層2との艶のコントラストにより、高い立体感が表出された意匠を有する。さらに、観察する角度によって意匠性が変化するような独特の意匠を表出する。 In the decorative molded product 10 of the present invention, the pattern layer 2 is provided on a part of the surface of the high-gloss-like molded product 1 and has a missing portion where the pattern layer 2 is not provided. For example, in the wood grain pattern, the conduit portion is missing from the pattern, and the pattern is provided in the other portion. Due to such a structure of the pattern layer, the decorative molded product 10 of the present invention has a high-gloss-like surface of the high-gloss-like molded product 1 which is a missing portion where the pattern layer 2 is not provided, and the gloss of the pattern layer 2. It has a design that expresses a high three-dimensional effect due to the contrast of. Furthermore, it expresses a unique design whose design changes depending on the observation angle.

なお、高艶調成形品1が、前述した基材層1aと高艶樹脂層1bとからなる場合は、図2に示すように、絵柄層2は、高艶樹脂層1b表面の一部に設けられる。 When the high-gloss molded product 1 is composed of the above-mentioned base material layer 1a and the high-gloss resin layer 1b, the pattern layer 2 is a part of the surface of the high-gloss resin layer 1b as shown in FIG. It will be provided.

絵柄層2は、通常、バインダー樹脂と着色剤とを含有する。絵柄層2のバインダー樹脂としては、熱可塑性樹脂が挙げられ、具体例としては、アクリル樹脂、アルキッドなどのポリエステル樹脂、不飽和ポリエステル樹脂、ウレタン樹脂(例えばポリエステルウレタン系樹脂)、ポリカーボネート樹脂、塩化ビニル-酢酸ビニル共重合体、ポリビニルブチラールなどのポリビニルアセタール(ブチラール系樹脂)、硝化綿などのニトロセルロース系樹脂が挙げられる。バインダー樹脂は、1種類単独で使用してもよいし、2種類以上を組み合わせて使用してもよい。 The pattern layer 2 usually contains a binder resin and a colorant. Examples of the binder resin of the pattern layer 2 include a thermoplastic resin, and specific examples thereof include acrylic resin, polyester resin such as alkyd, unsaturated polyester resin, urethane resin (for example, polyester urethane resin), polycarbonate resin, and vinyl chloride. -Vinyl acetate copolymer, polyvinyl acetal (butyral resin) such as polyvinyl butyral, and nitrocellulose resin such as nitrified cotton can be mentioned. One type of binder resin may be used alone, or two or more types may be used in combination.

着色剤としては、カーボンブラック(墨)、鉄黒、チタン白、アンチモン白、黄鉛、チタン黄、弁柄、カドミウム赤、群青、コバルトブルーなどの無機顔料、キナクリドンレッド、イソインドリノンイエロー、フタロシアニンブルーなどの有機顔料または染料、アルミニウム、真鍮などの鱗片状箔片からなる金属顔料、二酸化チタン被覆雲母、塩基性炭酸鉛などの鱗片状箔片からなる真珠光沢(パール)顔料などが用いられる。 Coloring agents include carbon black (black), iron black, titanium white, antimony white, yellow lead, titanium yellow, petals, cadmium red, ultramarine, cobalt blue and other inorganic pigments, quinacridone red, isoindolinone yellow, phthalocyanine. Organic pigments or dyes such as blue, metal pigments made of scaly foil pieces such as aluminum and brass, titanium dioxide-coated mica, and pearl gloss pigments made of scaly foil pieces such as basic lead carbonate are used.

絵柄層2の形成は、例えば、水圧転写法などの公知の方法で行うことができる。なかでも、高い立体感と、観察する角度によって意匠性が変化するような独特の意匠を表出した意匠を加飾成形品10に付与できる点で、絵柄層2は水圧転写法により形成されることが好ましい。 The pattern layer 2 can be formed by a known method such as a hydraulic transfer method. In particular, the pattern layer 2 is formed by the hydraulic transfer method in that a design expressing a unique design whose design changes depending on the observation angle can be imparted to the decorative molded product 10 with a high three-dimensional effect. Is preferable.

絵柄層2の厚みとしては、特に制限されないが、高い立体感と、観察する角度によって意匠性が変化するような独特の意匠を表出した意匠を加飾成形品10に付与する観点からは、好ましくは1~25μm程度、より好ましくは1~15μm程度が挙げられる。 The thickness of the pattern layer 2 is not particularly limited, but from the viewpoint of imparting a high three-dimensional effect and a design expressing a unique design whose design changes depending on the observation angle to the decorative molded product 10. It is preferably about 1 to 25 μm, and more preferably about 1 to 15 μm.

水圧転写法は、水圧転写フィルム20を用いて成形品を加飾する方法である。水圧転写フィルム20は、水溶性フィルム4と、上記水溶性フィルム4上に絵柄層2が設けられているフィルムであることが好ましい。本発明の加飾成形品10の絵柄層2は、水圧転写フィルムの絵柄層2が、高艶調成形品1上に転写されて形成されたものであることが好ましい。 The hydraulic transfer method is a method of decorating a molded product using the hydraulic transfer film 20. The hydraulic transfer film 20 is preferably a water-soluble film 4 and a film in which the pattern layer 2 is provided on the water-soluble film 4. The pattern layer 2 of the decorative molded product 10 of the present invention is preferably formed by transferring the pattern layer 2 of the hydraulic transfer film onto the high-gloss molded product 1.

図4は、水圧転写フィルムの一例の概略断面図を示す。図4に示すように、水圧転写フィルム20は、水溶性フィルム4上に、絵柄層2を備えたものである。 FIG. 4 shows a schematic cross-sectional view of an example of a hydraulic transfer film. As shown in FIG. 4, the hydraulic transfer film 20 is provided with a pattern layer 2 on a water-soluble film 4.

水溶性フィルム4を構成する樹脂としては、例えばポリビニルアルコール樹脂、デキストリン、ゼラチン、にかわ、カゼイン、セラック、アラビアゴム、澱粉、蛋白質、ポリアクリル酸アミド、ポリアクリル酸ナトリウム、ポリビニルメチルエーテル、メチルビニルエーテルと無水マレイン酸との共重合体、酢酸ビニルとイタコン酸との共重合体、ポリビニルピロリドン、アセチルセルロース、アセチルブチルセルロース、カルボキシメチルセルロース、メチルセルロース、ヒドロキシエチルセルロース、アルギン酸ナトリウムなどの各種水溶性ポリマーが挙げられる。これらの樹脂は、単独で用いられてもよいし、2種以上が混合されて用いられてもよい。なお、水溶性フィルム4には、マンナン、キサンタンガム、グアーガムなどのゴム成分が添加されていてもよい。 Examples of the resin constituting the water-soluble film 4 include polyvinyl alcohol resin, dextrin, gelatin, sardine, casein, cellac, gum arabic, starch, protein, polyacrylic acid amide, sodium polyacrylic acid, polyvinyl methyl ether, and methyl vinyl ether. Examples thereof include a copolymer with maleic anhydride, a copolymer of vinyl acetate and itaconic acid, and various water-soluble polymers such as polyvinylpyrrolidone, acetyl cellulose, acetyl butyl cellulose, carboxymethyl cellulose, methyl cellulose, hydroxyethyl cellulose, and sodium alginate. These resins may be used alone or in combination of two or more. A rubber component such as mannan, xanthan gum, or guar gum may be added to the water-soluble film 4.

水溶性フィルム4のうち、特に生産安定性と水に対する溶解性及び経済性の点から、ポリビニルアルコール(PVA)樹脂フィルムが好ましい。なお、ポリビニルアルコール樹脂フィルムは、PVA以外に、澱粉やゴムなどの添加剤を含有していてもよい。 Of the water-soluble films 4, polyvinyl alcohol (PVA) resin films are particularly preferable from the viewpoints of production stability, solubility in water, and economy. The polyvinyl alcohol resin film may contain additives such as starch and rubber in addition to PVA.

ポリビニルアルコール樹脂フィルムは、ポリビニルアルコールの重合度、ケン化度、及び澱粉やゴムなどの添加剤の配合量などを変えることにより、水溶性フィルム4に対して転写用の印刷層(絵柄層2)を形成する際に必要な機械的強度、取り扱い中の耐湿性、水面に浮かべてからの吸水による柔軟化の速度、水中での延展または拡散に要する時間、転写工程での変形のし易さなどを適宜調節することができる。 The polyvinyl alcohol resin film has a printing layer (picture layer 2) for transfer to the water-soluble film 4 by changing the degree of polymerization of polyvinyl alcohol, the degree of saponification, and the blending amount of additives such as starch and rubber. Mechanical strength required for forming, moisture resistance during handling, speed of softening by water absorption after floating on the water surface, time required for spreading or diffusion in water, ease of deformation in the transfer process, etc. Can be adjusted as appropriate.

ポリビニルアルコール樹脂フィルムからなる水溶性フィルム4として好適なものは、特開昭54-92406号公報に説明されているようなものであり、例えば、PVA樹脂80質量%、高分子水溶性樹脂15質量%、澱粉5質量%の混合組成からなり、平衡水分3%程度のものが好適である。 A suitable water-soluble film 4 made of a polyvinyl alcohol resin film is as described in Japanese Patent Application Laid-Open No. 54-92406, for example, 80% by mass of PVA resin and 15% by mass of polymer water-soluble resin. % And 5% by mass of starch, and the one having an equilibrium water content of about 3% is preferable.

また、ポリビニルアルコール樹脂フィルムは水溶性ではあるが、水に溶解する前段階では水に膨潤して軟化しつつもフィルムとして存続することが好ましい。フィルムとして存続している状態にあるときに水圧転写を行なうことにより、水圧転写時の転写用の印刷層の過度の流動、変形を防止することができるからである。 Although the polyvinyl alcohol resin film is water-soluble, it is preferable that the polyvinyl alcohol resin film remains as a film while swelling and softening in water before it is dissolved in water. This is because it is possible to prevent excessive flow and deformation of the print layer for transfer during hydraulic transfer by performing hydraulic transfer while the film is in a state of being alive.

水溶性フィルム4の厚さとしては、10~100μmが好ましい。10μm以上であると、フィルムの均一性が良好で、かつ生産安定性が高い。一方、100μm以下であると、水に対する溶解性が適度であり、かつ印刷適性に優れる。以上の観点から、水溶性フィルムの厚さは、20~60μmの範囲がより好ましい。 The thickness of the water-soluble film 4 is preferably 10 to 100 μm. When it is 10 μm or more, the uniformity of the film is good and the production stability is high. On the other hand, when it is 100 μm or less, the solubility in water is appropriate and the printability is excellent. From the above viewpoint, the thickness of the water-soluble film is more preferably in the range of 20 to 60 μm.

なお、水溶性フィルム4は、例えば紙、不織布、布などの水浸透性を有する基材と積層して使用することもできるが、このような水浸透性を有する基材と水溶性または水膨潤性を有する水溶性フィルム4とを積層したときには、水圧転写フィルム20を水面に浮かべる前に、水浸透性を有する基材を水溶性または水膨潤性を有する水溶性フィルム4から分離させるか、または水面に浮かべた後の水の作用によって水溶性または水膨潤性を有する水溶性フィルム4から水浸透性を有する基材が分離するように構成しておくことが好ましい。 The water-soluble film 4 can be used by laminating it with a water-permeable base material such as paper, non-woven fabric, or cloth, but it is water-soluble or water-swelling with such a water-permeable base material. When laminated with the water-soluble film 4 having properties, the water-permeable substrate is separated from the water-soluble or water-swellable water-soluble film 4 or separated from the water-soluble film 4 before floating the hydraulic transfer film 20 on the water surface. It is preferable that the base material having water permeability is separated from the water-soluble film 4 having water-soluble or water-swelling property by the action of water after floating on the water surface.

水圧転写フィルム20の絵柄層2の構成は、本発明の加飾成形品10の絵柄層2と同様の構成であることが好ましい。 The structure of the pattern layer 2 of the hydraulic transfer film 20 is preferably the same as that of the pattern layer 2 of the decorative molded product 10 of the present invention.

水圧転写フィルム20は、上記水溶性フィルム4上に、絵柄層2を構成する塗工液を用いて公知の塗布方法または印刷方法により、あるいは樹脂フィルムをラミネートすることにより絵柄層2を形成して、製造することができる。上記塗布方法としては、グラビアコート、リバースコート等が挙げられ、印刷方法としては、グラビア印刷等が挙げられる。 The hydraulic transfer film 20 forms the pattern layer 2 on the water-soluble film 4 by a known coating method or printing method using the coating liquid constituting the pattern layer 2, or by laminating a resin film. , Can be manufactured. Examples of the coating method include gravure coating and reverse coating, and examples of the printing method include gravure printing.

水圧転写フィルム20を用いた絵柄層2の具体的な形成方法については、後段の本発明の加飾成形品の製造方法の項において述べる。 A specific method for forming the pattern layer 2 using the hydraulic transfer film 20 will be described later in the section of the method for manufacturing a decorative molded product of the present invention.

<トップコート層3>
本発明の加飾成形品10は、絵柄層2上に、トップコート層3をさらに有していてもよい。トップコート層3を有することにより、絵柄層2を保護したり、表面強度を高めたり、表面の艶を調整することができる。
<Top coat layer 3>
The decorative molded product 10 of the present invention may further have a top coat layer 3 on the pattern layer 2. By having the top coat layer 3, it is possible to protect the pattern layer 2, increase the surface strength, and adjust the gloss of the surface.

図3は、絵柄層2上にトップコート層3を有する、本発明の加飾成形品10の構成の一例を示す概略断面図である。 FIG. 3 is a schematic cross-sectional view showing an example of the configuration of the decorative molded product 10 of the present invention, which has the top coat layer 3 on the pattern layer 2.

トップコート層3を形成する材料としては、例えば、熱可塑性樹脂、熱硬化性樹脂、紫外線硬化性樹脂などが選択され、具体的には、ウレタン系樹脂、エポキシ樹脂、アクリル系樹脂、フッ素系樹脂、ケイ素系樹脂などが挙げられる。 As the material for forming the top coat layer 3, for example, a thermoplastic resin, a thermosetting resin, an ultraviolet curable resin, or the like is selected, and specifically, a urethane resin, an epoxy resin, an acrylic resin, a fluororesin, or the like is selected. , Silicon-based resin and the like.

トップコート層3の形成は、前述の樹脂を公知の有機溶剤に溶解して得た塗料を用いて、スプレー塗装、静電塗装、刷毛塗り、浸漬塗装、など公知の塗装方法により行うことができる。 The top coat layer 3 can be formed by a known coating method such as spray coating, electrostatic coating, brush coating, dip coating, etc., using a coating material obtained by dissolving the above-mentioned resin in a known organic solvent. ..

トップコート層3は、艶消し調であってもよい。トップコート層3が艶消し調である場合、トップコート層3は、艶消し剤を含んでいることが好ましい。 The top coat layer 3 may have a matte tone. When the top coat layer 3 has a matte tone, it is preferable that the top coat layer 3 contains a matting agent.

艶消し剤としては、例えば、シリカ、クレー、重質炭酸カルシウム、軽質炭酸カルシウム、沈降性硫酸バリウム、ケイ酸カルシウム、合成ケイ酸塩、及びケイ酸微粉末から選択される無機フィラーや、アクリル樹脂、ウレタン樹脂、ナイロン樹脂、ポリプロピレン樹脂、または尿素系樹脂から選択される有機フィラーまたは樹脂ビーズが挙げられ、いずれか1種を用いてもよいし、2種以上を組み合わせて用いることもできる。これらの中でも、高い立体感と、観察する角度によって意匠性が変化するような独特の意匠を加飾成形品10に付与する観点からは、好ましくはシリカ、炭酸カルシウム、沈降性バリウムが挙げられ、より好ましくはシリカが挙げられる。 As the matting agent, for example, an inorganic filler selected from silica, clay, heavy calcium carbonate, light calcium carbonate, precipitated barium sulfate, calcium silicate, synthetic silicate, and fine powder of silicate, and an acrylic resin. , Urethane resin, nylon resin, polypropylene resin, or urea-based resin, organic fillers or resin beads may be used, and any one of them may be used, or two or more of them may be used in combination. Among these, silica, calcium carbonate, and sedimentary barium are preferable from the viewpoint of imparting a high three-dimensional effect and a unique design whose design changes depending on the observation angle to the decorative molded product 10. More preferably, silica is mentioned.

艶消し剤の体積平均粒径は、好ましくは0.5~25μmであり、より好ましくは1~15μm、さらに好ましくは1~10μm、さらにより好ましくは1~5μm、特に好ましくは1~3μmである。艶消し剤の体積平均粒径が25μm以下であれば、界面積が増大することによって加工時の応力が拡散し、界面に発生したボイド等がエネルギーを吸収したり、粒子間距離が小さくなることによって粒子、またはボイド間で塑性変形が生じ、伸張時の白化を抑制することができる。また、艶消し剤の体積平均粒径が0.5μm以上であると、艶消し効果の観点から好ましい。なお、ここで言う体積平均粒径は、レーザー回折-散乱法によって求めた粒度分布における積算値50%での粒径である。 The volume average particle size of the matting agent is preferably 0.5 to 25 μm, more preferably 1 to 15 μm, still more preferably 1 to 10 μm, still more preferably 1 to 5 μm, and particularly preferably 1 to 3 μm. .. If the volume average particle size of the matting agent is 25 μm or less, the stress during processing is diffused due to the increase in the boundary area, the voids generated at the interface absorb energy, and the distance between particles becomes small. Causes plastic deformation between particles or voids, and whitening during stretching can be suppressed. Further, it is preferable that the volume average particle size of the matting agent is 0.5 μm or more from the viewpoint of the matting effect. The volume average particle size referred to here is the particle size at an integrated value of 50% in the particle size distribution obtained by the laser diffraction-scattering method.

艶消し剤のJIS K 5101-13-1:2004に準拠して測定した吸油量としては、230mL/100g以上、好ましくは230~400mL/100gであり、230~350mL/100gであることがより好ましく、230~300mL/100gであることがさらに好ましい。吸油量が230mL/100g以上の艶消し剤を用いることが艶消し効果の観点から好ましく、また吸油量が400mL/100g以下の艶消し剤を用いることが、艶消し剤を塗工液に適用する場合、適度なチキソ性を維持して塗工適性を損なわないとの観点から好ましい。 The oil absorption measured in accordance with JIS K 5101-13-1: 2004 of the matting agent is 230 mL / 100 g or more, preferably 230 to 400 mL / 100 g, and more preferably 230 to 350 mL / 100 g. , 230-300 mL / 100 g, more preferably. It is preferable to use a matting agent having an oil absorption amount of 230 mL / 100 g or more from the viewpoint of the matting effect, and it is preferable to use a matting agent having an oil absorption amount of 400 mL / 100 g or less to apply the matting agent to the coating liquid. In this case, it is preferable from the viewpoint of maintaining an appropriate thixotropic property and not impairing the coating suitability.

なお、上記艶消し剤は、表面処理をしたものであってもよい。このような表面処理は成形加工時のクラックや白化を抑制できるため好ましい。処理の手法としては、上記効果を奏するものであれば特に制限はなく、有機材料による表面処理であっても、無機材料による表面処理であってもよい。特に、シランカップリング処理などが好適に挙げられる。 The matting agent may be surface-treated. Such surface treatment is preferable because it can suppress cracks and whitening during molding. The treatment method is not particularly limited as long as it exhibits the above effects, and may be a surface treatment using an organic material or a surface treatment using an inorganic material. In particular, a silane coupling treatment or the like is preferably mentioned.

トップコート層3が艶消し剤を含む場合、トップコート層に4おける艶消し剤の含有量としては、好ましくは1~40質量%程度、より好ましくは20~40質量%程度が挙げられる。 When the top coat layer 3 contains a matting agent, the content of the matting agent in the top coat layer 4 is preferably about 1 to 40% by mass, more preferably about 20 to 40% by mass.

トップコート層3の厚みとしては、特に制限されず、好ましくは1~25μmであり、より好ましくは1~15μmである。 The thickness of the top coat layer 3 is not particularly limited, and is preferably 1 to 25 μm, more preferably 1 to 15 μm.

[加飾成形品の製造方法]
本発明の加飾成形品を製造する方法としては、特に制限されないが、水溶性フィルムと、水溶性フィルム上の一部に設けられた絵柄層とを有する水圧転写フィルムを用いて、高艶調成形品上に絵柄層を転写する工程を有する水圧転写法が好適である。
[Manufacturing method of decorative molded products]
The method for producing the decorative molded product of the present invention is not particularly limited, but a high gloss tone is used by using a water-soluble film and a hydraulic transfer film having a pattern layer provided on a part of the water-soluble film. A hydraulic transfer method including a step of transferring a pattern layer onto a molded product is suitable.

水溶性フィルム4と、水溶性フィルム4上の一部に設けられた絵柄層2とを有する水圧転写フィルム20については、前述の通りである。 The hydraulic transfer film 20 having the water-soluble film 4 and the pattern layer 2 provided on a part of the water-soluble film 4 is as described above.

水圧転写フィルム20を用いて、高艶調成形品1上に絵柄層2を転写する工程は、具体的には、以下の工程(a)から工程(d)を含む。
すなわち、本発明の加飾成形品10は、具体的には、以下の工程(a)から工程(d)を含む方法により、好適に製造することができる。
工程(a)水圧転写フィルムを、水溶性フィルム側が下向きで水面側に向くように水面に浮遊させる工程
工程(b)上記水圧転写フィルムの絵柄層側に活性剤組成物を塗布する活性剤塗布工程
工程(c)該工程(a)及び(b)を経た、水面に浮遊している水圧転写フィルム上に高艶調成形品を押圧し、水圧によって上記絵柄層を高艶調成形品の高艶調表面に密着させる工程
工程(d)高艶調成形品の高艶調表面に密着した水溶性フィルムを除去する脱膜工程
Specifically, the step of transferring the pattern layer 2 onto the high-gloss-like molded product 1 using the hydraulic transfer film 20 includes the following steps (a) to (d).
That is, the decorative molded product 10 of the present invention can be suitably manufactured by a method including the following steps (a) to (d).
Step (a) A step of suspending the hydraulic transfer film on the water surface so that the water-soluble film side faces downward and the water surface side. Step (b) An activator coating step of applying the active agent composition to the pattern layer side of the hydraulic transfer film. Step (c) The high-gloss-like molded product is pressed onto the hydraulic transfer film floating on the water surface after the steps (a) and (b), and the pattern layer is subjected to the high-gloss-like molded product by water pressure. Step to make it adhere to the toned surface Step (d) Defilming step to remove the water-soluble film that adheres to the toned surface of the high-gloss-like molded product

また、上記工程(d)に次いで、下記の工程(e)を備えていてもよい。
工程(e):高艶調成形品上に形成された絵柄層の上に、トップコート層を形成する工程
Further, following the above step (d), the following step (e) may be provided.
Step (e): A step of forming a top coat layer on a pattern layer formed on a high-gloss molded product.

<工程(a)>
工程(a)は、工程(b)の前または後に行うことができる。工程(a)では、水圧転写フィルム20を、水溶性フィルム4側が下向きで水面側に向くように水面上に浮遊させる。水圧転写フィルム20を水面に浮遊させるには、枚葉の印刷物を1枚ずつ浮遊させてもよく、また水を一方向に流し、その水面上に連続帯状の水圧転写フィルム20を、連続的に供給して浮遊させてもよい。
<Step (a)>
Step (a) can be performed before or after step (b). In the step (a), the hydraulic transfer film 20 is suspended on the water surface so that the water-soluble film 4 side faces downward and faces the water surface side. In order to suspend the hydraulic transfer film 20 on the water surface, the sheet-fed printed matter may be suspended one by one, or water is allowed to flow in one direction, and a continuous band-shaped hydraulic transfer film 20 is continuously formed on the water surface. It may be supplied and floated.

<工程(b)>
工程(b)は、工程(a)の前または後に行うことができ、水圧転写フィルム20の絵柄層2側に活性剤組成物を塗布する工程である。この工程で活性剤組成物を塗布することにより、絵柄層2の少なくとも一部が溶解乃至膨潤して軟化し(活性化し)、被転写体である高艶調成形品1と密着しやすくなる。
<Step (b)>
The step (b) can be performed before or after the step (a), and is a step of applying the activator composition to the pattern layer 2 side of the hydraulic transfer film 20. By applying the activator composition in this step, at least a part of the pattern layer 2 is dissolved or swollen and softened (activated), and it becomes easy to adhere to the high-gloss-like molded product 1 which is the transferred product.

(活性剤組成物)
絵柄層2に塗布する活性剤組成物は、絵柄層2を活性化して、被転写体(すなわち、高艶調成形品1)の被転写面(すなわち、高艶調表面)に転写させる機能を有する組成物であれば特に制限はなく、また、被転写体の被転写面に各層を転写させるまで蒸発しないような性状を有することが好ましい。このような活性剤組成物としては、例えばエステル類、アセチレングリコール類、エーテル類、及び樹脂を含む組成物が好ましく挙げられる。
(Activator composition)
The activator composition applied to the pattern layer 2 has a function of activating the pattern layer 2 and transferring it to the transferred surface (that is, the highly glossy surface) of the transferred body (that is, the high gloss tone molded product 1). The composition is not particularly limited as long as it has, and it is preferable that the composition has a property that it does not evaporate until each layer is transferred to the surface to be transferred. Preferred examples of such an activator composition include compositions containing esters, acetylene glycols, ethers, and resins.

エステル類としては、酢酸エチル、酢酸プロピル、酢酸ブチル、酢酸イソブチル、酢酸sec-ブチル、酢酸tert-ブチル、シュウ酸ジブチル、フタル酸ジブチル、フタル酸ジメチル、フタル酸ジオクチル、フタル酸ジイソオクチルなどが好ましく挙げられる。アセチレングリコール類としては、メトキシブチルアセテート、エトキシブチルアセテート、エチルカルビトールアセテート、プロピルカルビトールアセテート、ブチルカルビトールアセテートなどが好ましく挙げられる。エーテル類としては、メチルセロソルブ、ブチルセロソルブ、イソアミルセロソルブなどが好ましく挙げられる。 Preferred examples of the esters include ethyl acetate, propyl acetate, butyl acetate, isobutyl acetate, sec-butyl acetate, tert-butyl acetate, dibutyl acetate, dibutyl phthalate, dimethyl phthalate, dioctyl phthalate, and diisooctyl phthalate. Be done. Preferred examples of acetylene glycols include methoxybutyl acetate, ethoxybutyl acetate, ethyl carbitol acetate, propyl carbitol acetate, and butyl carbitol acetate. Preferred examples of ethers include methyl cellosolve, butyl cellosolve, and isoamyl cellosolve.

また、樹脂としては、アクリレート系単量体の単独または共重合体などの熱可塑性樹脂や、ポリアミド樹脂、ポリエステル樹脂、フェノール樹脂、メラミン樹脂、尿素樹脂、エポキシ樹脂、フタル酸アルキッド樹脂、フタル酸ジアリル樹脂、アルキッド樹脂、ポリウレタン樹脂などの熱硬化性樹脂などが好ましく挙げられ、なかでも熱硬化性樹脂が好ましい。 Further, as the resin, a thermoplastic resin such as an acrylate-based monomer alone or a copolymer, a polyamide resin, a polyester resin, a phenol resin, a melamine resin, a urea resin, an epoxy resin, an alkyd phthalate resin, and a diallyl phthalate are used. Thermally curable resins such as resins, alkyd resins, and polyurethane resins are preferred, with thermocurable resins being preferred.

本発明で用いられる活性剤組成物の好ましい各組成の含有量は、エステル類では5~40質量%、アセチレングリコール類では40~80質量%、エーテル類では5~30質量%、及び樹脂では1~20質量%程度である。 The content of each preferable composition of the activator composition used in the present invention is 5 to 40% by mass for esters, 40 to 80% by mass for acetylene glycols, 5 to 30% by mass for ethers, and 1 for resins. It is about 20% by mass.

活性剤組成物の塗布は、グラビア印刷やスプレーコート法などにより行えばよく、その塗布量は通常1~50g/m2であり、好ましくは3~30g/m2であり、さらに好ましくは10~20g/m2である。 The activator composition may be applied by gravure printing, a spray coating method, or the like, and the amount of the activator composition is usually 1 to 50 g / m 2 , preferably 3 to 30 g / m 2 , and more preferably 10 to 10. It is 20 g / m 2 .

<工程(c)>
工程(c)は、工程(a)及び工程(b)を経た、水面に浮遊している水圧転写フィルム20上に被転写体である高艶調成形品1を押圧し、水圧によって水圧転写フィルム20の絵柄層2を高艶調成形品1の高艶調表面に密着させる工程である。なお、高艶調成形品1が高艶樹脂層1bを有する場合は、被転写面は高艶樹脂層1bの表面となる。水圧転写フィルム20を浮かべ水圧を印加するための水は、該水圧転写フィルム20の水溶性フィルム4の種類などに応じ、適宣水温を調整するのがよく、好ましくは25~50℃程度、より好ましくは25~35℃である。
<Step (c)>
In the step (c), the high-gloss-like molded product 1 to be transferred is pressed onto the hydraulic transfer film 20 floating on the water surface after the steps (a) and (b), and the hydraulic transfer film is subjected to hydraulic pressure. This is a step of bringing the pattern layer 2 of 20 into close contact with the high-gloss surface of the high-gloss molded product 1. When the high-gloss molded product 1 has the high-gloss resin layer 1b, the surface to be transferred is the surface of the high-gloss resin layer 1b. The water for floating the hydraulic transfer film 20 and applying the hydraulic pressure is preferably adjusted to an appropriate water temperature according to the type of the water-soluble film 4 of the hydraulic transfer film 20, preferably about 25 to 50 ° C., and more. It is preferably 25 to 35 ° C.

また、本発明の水圧転写フィルム20と高艶調成形品1との転写時間は、20~120秒程度が好ましく、より好ましくは30~60秒程度である。 The transfer time between the hydraulic transfer film 20 of the present invention and the high-gloss molded product 1 is preferably about 20 to 120 seconds, more preferably about 30 to 60 seconds.

工程(c)において、絵柄層2に塗布した活性剤組成物は高艶調成形品1と接し、該高艶調成形品1の表面を溶解させることで、水圧転写フィルム20と高艶調成形品1との密着性をさらに良好なものとすることができる。 In the step (c), the activator composition applied to the pattern layer 2 is in contact with the high-gloss-like molded product 1 and the surface of the high-gloss-like molded product 1 is dissolved to dissolve the hydraulic transfer film 20 and the high-gloss-like molding. The adhesion with the product 1 can be further improved.

<工程(d)>
工程(d)は、工程(c)の後に行われ、高艶調成形品1の被転写面(高艶調表面)に密着した水溶性フィルム4を除去する工程である。高艶調成形品1の被転写面上に付着している水溶性フィルム4の除去は、例えば、水を用いてシャワー洗浄することで行うことができる。なお、シャワー洗浄の条件は、水溶性フィルム4を形成する材料などにより異なるが、通常は水温15~60℃程度、洗浄時間10秒~5分程度が好ましい。そして、工程(d)の後、被転写体を十分乾燥し水分を蒸発させる。
<Step (d)>
The step (d) is performed after the step (c) and is a step of removing the water-soluble film 4 in close contact with the transferred surface (high gloss tone surface) of the high gloss tone molded product 1. The water-soluble film 4 adhering to the surface to be transferred of the high-gloss molded product 1 can be removed by, for example, shower washing with water. The conditions for shower cleaning vary depending on the material forming the water-soluble film 4, but usually the water temperature is preferably about 15 to 60 ° C. and the washing time is preferably about 10 seconds to 5 minutes. Then, after the step (d), the transferred body is sufficiently dried to evaporate the water content.

以上の工程(a)~(d)により、本発明の加飾成形品10を製造することができる。 By the above steps (a) to (d), the decorative molded product 10 of the present invention can be manufactured.

<工程(e)>
工程(e)は、高艶調成形品1上に形成された絵柄層2上に、必要に応じトップコート層3を形成する工程である。工程(e)を行う場合、当該工程(e)においては、絵柄層2に対し、表面強度の向上、表面保護、表面の艶調整などのために必要に応じ塗装を施し、透明ないし半透明のトップコート層3を形成する。
<Step (e)>
The step (e) is a step of forming the top coat layer 3 on the pattern layer 2 formed on the high-gloss molded product 1 as needed. When the step (e) is performed, in the step (e), the pattern layer 2 is coated as necessary for improving the surface strength, protecting the surface, adjusting the gloss of the surface, etc., and is transparent or translucent. The top coat layer 3 is formed.

このトップコート層3を形成する材料としては、例えば熱可塑性樹脂、熱硬化性樹脂、紫外線硬化性樹脂などが選択され、具体的にはウレタン系樹脂、エポキシ樹脂、アクリル系樹脂、フッ素系樹脂、ケイ素系樹脂などが用いられる。トップコート層3の形成は、上記の樹脂を公知の有機溶剤に溶解して得た塗料を用いて、スプレー塗装、静電塗装、刷毛塗り、浸漬塗装、など公知の塗装方法により行うことができる。また、トップコート層の厚みは、好ましくは1~25μmであり、より好ましくは1~10μmである。 As a material for forming the top coat layer 3, for example, a thermoplastic resin, a thermosetting resin, an ultraviolet curable resin or the like is selected, and specifically, a urethane resin, an epoxy resin, an acrylic resin, a fluororesin, etc. Silicon-based resin or the like is used. The top coat layer 3 can be formed by a known coating method such as spray coating, electrostatic coating, brush coating, dip coating, etc., using a coating material obtained by dissolving the above resin in a known organic solvent. .. The thickness of the top coat layer is preferably 1 to 25 μm, more preferably 1 to 10 μm.

次に、本発明を実施例により、さらに詳細に説明するが、本発明は、これらの例によってなんら限定されるものではない。なお、実施例及び比較例において測定したグロス値(60°)は、市販のグロスメーターを用いて、艶消調成形品の表面に対する光の入射角60°の条件として測定されたグロス値であり、任意の3点を測定した平均値である。 Next, the present invention will be described in more detail by way of examples, but the present invention is not limited to these examples. The gloss value (60 °) measured in Examples and Comparative Examples is a gloss value measured using a commercially available gloss meter under the condition that the angle of incidence of light on the surface of the matte molded product is 60 °. , Is the average value measured at any three points.

<水圧転写フィルムの製造例>
水溶性フィルムとして、ポリビニルアルコール(PVA)フィルム(厚さ40μm)を用い、その片面に、硝化綿とアルキッド樹脂とを80:20の質量比で含む下記のインキを用いて、グラビア印刷により、導管部分が抜けであり、それ以外の部分が絵柄である木目模様を有する絵柄層(厚さ3μm)を形成し、水溶性フィルム/絵柄層が積層された水圧転写フィルムを得た。
(絵柄層を形成するインキ)
硝化綿とアルキド樹脂とを80:20の質量比で含み、着色剤として弁柄及びカーボンブラックを所定の配合比率で使用した着色インキ。
<Manufacturing example of hydraulic transfer film>
A polyvinyl alcohol (PVA) film (thickness 40 μm) is used as the water-soluble film, and the following ink containing vitrified cotton and alkyd resin in a mass ratio of 80:20 is used on one side thereof, and the conduit is subjected to gravure printing. A pattern layer (thickness 3 μm) having a wood grain pattern in which the portion was missing and the other portion was a pattern was formed, and a water-soluble film / pattern layer was laminated to obtain a hydraulic transfer film.
(Ink that forms the pattern layer)
A colored ink containing nitrocellulose and alkyd resin in a mass ratio of 80:20, and using a valve handle and carbon black as a coloring agent in a predetermined blending ratio.

<高艶調成形品Aの製造>
基材層としてのABS樹脂板(厚み2mm、表面のグロス値(60°)は60)の上に、アクリルポリマーポリオール(重量平均分子量:30,000、水酸基価:80mgKOH/g)とウレタンウレア樹脂(ガラス転移点:40℃、水酸基価:1mgKOH/g未満)との質量比8:2の混合樹脂を含むインキを塗工し、厚さ15μmの高艶樹脂層を形成した。得られた高艶調成形品Aの表面のグロス値(60°)は、90であった。
<Manufacturing of high-gloss molded product A>
Acrylic polymer polyol (weight average molecular weight: 30,000, hydroxyl value: 80 mgKOH / g) and urethane urea resin on an ABS resin plate (thickness 2 mm, surface gloss value (60 °) is 60) as a base material layer. An ink containing a mixed resin having a mass ratio of 8: 2 with (glass transition point: 40 ° C., hydroxyl value: less than 1 mgKOH / g) was applied to form a high gloss resin layer having a thickness of 15 μm. The gloss value (60 °) on the surface of the obtained high-gloss molded product A was 90.

<高艶調成形品Bの製造>
高艶調成形品Aの製造において、高艶樹脂層の厚さを10μmとした以外は、高艶調成形品Aの製造と同様にして、高艶調成形品Bを調製した。得られた高艶調成形品Bの表面のグロス値(60°)は、80であった。
<Manufacturing of high-gloss molded product B>
In the production of the high-gloss-like molded product A, the high-gloss-like molded product B was prepared in the same manner as in the production of the high-gloss-like molded product A, except that the thickness of the high-gloss resin layer was 10 μm. The gloss value (60 °) on the surface of the obtained high-gloss molded product B was 80.

<高艶調成形品Cの製造>
高艶調成形品Aの製造において、高艶樹脂層の厚さを5μmとした以外は、高艶調成形品Aの製造と同様にして、高艶調成形品Cを調製した。得られた高艶調成形品Cの表面のグロス値(60°)は、70であった。
<Manufacturing of high-gloss molded product C>
In the production of the high-gloss-like molded product A, the high-gloss-like molded product C was prepared in the same manner as in the production of the high-gloss-like molded product A, except that the thickness of the high-gloss resin layer was set to 5 μm. The gloss value (60 °) on the surface of the obtained high-gloss molded product C was 70.

<成形品D>
成形品Dとして、上記のABS樹脂板(厚み2mm、表面のグロス値(60°)は60)をそのまま用いた。
<Molded product D>
As the molded product D, the above ABS resin plate (thickness 2 mm, surface gloss value (60 °) is 60) was used as it was.

<実施例1> 加飾成形品Aの製造
上記で得られた水圧転写フィルムの絵柄層表面に、下記組成の活性剤組成物を10g/m2塗布し、スムージングロールで上記活性剤組成物を均一にした後、水溶性フィルム側
が下向きで水面側を向くように水圧転写フィルムを水面に浮遊させた。次いで、浮遊した水圧転写フィルムに、上記の高艶調成形品Aを、高艶樹脂層が水面側になるようにして押圧し、水圧によって絵柄層を高艶調成形品1の高艶樹脂層面に密着させる工程、及び、水洗により水溶性フィルムを除去する脱膜工程を経た。次に、絵柄層上に2液硬化タイプのウレタン樹脂の塗料(シリカ20質量%含有)をスプレー塗装することにより、厚み15μmのトップコート層を形成し、加飾成形品Aを得た。
<Example 1> Production of decorative molded product A 10 g / m 2 of the activator composition having the following composition is applied to the surface of the pattern layer of the hydraulic transfer film obtained above, and the activator composition is applied by a smoothing roll. After making the film uniform, the hydraulic transfer film was suspended on the water surface so that the water-soluble film side was facing downward and the water surface side was facing. Next, the above-mentioned high-gloss-like molded product A is pressed against the floating hydraulic transfer film so that the high-gloss resin layer is on the water surface side, and the pattern layer is pressed by water pressure on the high-gloss resin layer surface of the high-gloss-like molded product 1. A step of bringing the film into close contact with the film and a step of removing the water-soluble film by washing with water were performed. Next, a two-component curing type urethane resin paint (containing 20% by mass of silica) was spray-coated on the pattern layer to form a top coat layer having a thickness of 15 μm, and a decorative molded product A was obtained.

(活性剤組成物の組成)
フタル酸系アルキッド樹脂 6質量部
マイクロシリカ(顔料) 2質量部
フタル酸ジブチル 17質量部
溶剤(ブチルカルビトールアセテート) 60質量部
溶剤(ブチルセロソルブ) 15質量部
(Composition of activator composition)
Phthalic acid-based alkyd resin 6 parts by mass Micro silica (pigment) 2 parts by mass Dibutyl phthalate 17 parts by mass Solvent (butyl carbitol acetate) 60 parts by mass Solvent (butyl cellosolve) 15 parts by mass

<実施例2> 加飾成形品Bの製造
実施例1において、高艶調成形品Aの代わりに高艶調成形品Bを用いた以外は、実施例1と同様にして、加飾成形品Bを得た。
<Example 2> Production of decorative molded product B The decorative molded product is the same as in Example 1 except that the high-gloss-like molded product B is used instead of the high-gloss-like molded product A in Example 1. B was obtained.

<実施例3> 加飾成形品Cの製造
実施例1において、高艶調成形品Aの代わりに高艶調成形品Cを用いた以外は、実施例1と同様にして、加飾成形品Cを得た。
<Example 3> Production of decorative molded product C The decorative molded product is the same as in Example 1 except that the high-gloss-like molded product C is used instead of the high-gloss-like molded product A in Example 1. C was obtained.

<比較例1> 加飾成形品Dの製造
実施例1において、高艶調成形品Aの代わりに成形品Dを用いた以外は、実施例1と同様にして、加飾成形品Dを得た。
<Comparative Example 1> Production of Decorative Molded Product D A decorative molded product D is obtained in the same manner as in Example 1 except that the molded product D is used instead of the high gloss-like molded product A in Example 1. rice field.

意匠性評価1
上記で得られた加飾成形品を目視により観察し、その意匠性について以下の基準で評価した。結果を表1に示す。
◎:全体に艶消し調で抜け導管部分が絵柄部分よりも艶が高いことによる高い立体感と深みのある意匠がかなり強く表現されている。
○:全体に艶消し調で抜け導管部分が絵柄部分よりも艶が高いことによる高い立体感と深みのある意匠が強く表現されている。
△:全体に艶消し調で抜け導管部分が絵柄部分よりも艶が高いことによる高い立体感と深みのある意匠がやや表現されている。
×:全体に艶消し調で抜け導管部分が絵柄部分よりも艶が高いことによる高い立体感と深みのある意匠が表現されていない。
Design evaluation 1
The decorative molded product obtained above was visually observed and its design was evaluated according to the following criteria. The results are shown in Table 1.
⊚: The overall design is matte and the conduit part is glossier than the pattern part, which gives a high three-dimensional effect and a deep design.
◯: The overall design is matte and the conduit part is glossier than the pattern part, which strongly expresses a high three-dimensional effect and a deep design.
Δ: The overall design is matte and the conduit part is glossier than the pattern part, which gives a high three-dimensional effect and a deep design.
X: The overall design is matte and the conduit part is glossier than the pattern part, which does not express a high three-dimensional effect and a deep design.

意匠性評価2
上記で得られた加飾成形品を目視により観察し、その意匠性について以下の基準で評価した。結果を表1に示す。
◎:加飾成形品を水平方向、45度方向、垂直方向から観察した場合に、それぞれの角度における意匠に変化がある。
〇:加飾成形品を水平方向から観察した場合のみ、45度方向及び垂直方向から観察した場合と意匠に変化がある。
△:加飾成形品を水平方向から観察した場合のみ、45度方向及び垂直方向から観察した場合と意匠に若干の変化がある。
×:加飾成形品を水平方向、45度方向、垂直方向から観察した場合に、それぞれの角度における意匠に変化がない。
Design evaluation 2
The decorative molded product obtained above was visually observed and its design was evaluated according to the following criteria. The results are shown in Table 1.
⊚: When the decorative molded product is observed from the horizontal direction, the 45 degree direction, and the vertical direction, there is a change in the design at each angle.
〇: There is a change in the design only when the decorative molded product is observed from the horizontal direction and when it is observed from the 45 degree direction and the vertical direction.
Δ: There is a slight change in the design only when the decorative molded product is observed from the horizontal direction and when it is observed from the 45 degree direction and the vertical direction.
X: When the decorative molded product is observed from the horizontal direction, the 45 degree direction, and the vertical direction, there is no change in the design at each angle.

Figure 0007067542000001
Figure 0007067542000001

1 高艶調成形品
1a 基材層
1b 高艶樹脂層
2 絵柄層
10 加飾成形品
3 トップコート層
20 水圧転写フィルム
4 水溶性フィルム
1 High-gloss molded product 1a Base material layer 1b High-gloss resin layer 2 Picture layer 10 Decorative molded product 3 Top coat layer 20 Hydraulic transfer film 4 Water-soluble film

Claims (7)

高艶調成形品と、前記高艶調成形品表面に設けられた絵柄層とを有し、
前記絵柄層は、前記高艶調成形品表面の一部に設けられ、前記絵柄層が設けられていない抜けの部分を有しており、
前記高艶調成形品は、基材層と、高艶樹脂層との積層体であり、
前記基材層は、樹脂により構成されており、
前記高艶調成形品は、前記絵柄層側の表面のグロス値(60°)が70以上95以下である、加飾成形品。
It has a high-gloss-like molded product and a pattern layer provided on the surface of the high-gloss-like molded product.
The pattern layer is provided on a part of the surface of the high-gloss molded product, and has a missing portion where the pattern layer is not provided.
The high-gloss molded product is a laminate of a base material layer and a high-gloss resin layer.
The base material layer is made of resin and is made of resin.
The high-gloss molded product is a decorative molded product in which the gloss value (60 °) of the surface on the pattern layer side is 70 or more and 95 or less.
記高艶樹脂層が前記絵柄層側に積層されている、請求項1に記載の加飾成形品。 The decorative molded product according to claim 1, wherein the high-gloss resin layer is laminated on the pattern layer side. 前記高艶樹脂層は、アクリルポリマーポリオールを含む樹脂組成物の硬化物により形成されている、請求項2に記載の加飾成形品。 The decorative molded product according to claim 2, wherein the high-gloss resin layer is formed of a cured product of a resin composition containing an acrylic polymer polyol. 前記絵柄層上にトップコート層をさらに有する、請求項1~3のいずれかに記載の加飾成形品。 The decorative molded product according to any one of claims 1 to 3, further comprising a top coat layer on the pattern layer. 前記トップコート層は、艶消し調である、請求項4に記載の加飾成形品。 The decorative molded product according to claim 4, wherein the top coat layer has a matte tone. 高艶調成形品と、前記高艶調成形品表面に設けられた絵柄層とを有する、加飾成形品の製造方法であって、
前記絵柄層は、前記高艶調成形品表面の一部に設けられ、前記絵柄層が設けられていない抜けの部分を有しており、
前記高艶調成形品は、基材層と、高艶樹脂層との積層体であり、
前記基材層は、樹脂により構成されており、
前記高艶調成形品は、前記絵柄層側の表面のグロス値(60°)が70以上95以下であり、
水溶性フィルムと、前記水溶性フィルム上の一部に設けられた絵柄層とを有する水圧転写フィルムを用いて、高艶調成形品上に絵柄層を転写する工程を備える、加飾成形品の製造方法。
A method for manufacturing a decorative molded product, which has a high-gloss-like molded product and a pattern layer provided on the surface of the high-gloss-like molded product.
The pattern layer is provided on a part of the surface of the high-gloss molded product, and has a missing portion where the pattern layer is not provided.
The high-gloss molded product is a laminate of a base material layer and a high-gloss resin layer.
The base material layer is made of resin and is made of resin.
The high-gloss molded product has a gloss value (60 °) of the surface on the pattern layer side of 70 or more and 95 or less.
A decorative molded product comprising a step of transferring a pattern layer onto a high-gloss-like molded product using a hydraulic transfer film having a water-soluble film and a pattern layer provided on a part of the water-soluble film. Production method.
記高艶樹脂層が前記絵柄層側に積層されている、請求項6に記載の加飾成形品の製造方法。
The method for manufacturing a decorative molded product according to claim 6, wherein the high-gloss resin layer is laminated on the pattern layer side.
JP2019201122A 2019-11-06 2019-11-06 Decorative molded products and their manufacturing methods Active JP7067542B2 (en)