JP6903804B1 - Flexible image display device and optical laminate used for it - Google Patents

Flexible image display device and optical laminate used for it Download PDF

Info

Publication number
JP6903804B1
JP6903804B1 JP2020159585A JP2020159585A JP6903804B1 JP 6903804 B1 JP6903804 B1 JP 6903804B1 JP 2020159585 A JP2020159585 A JP 2020159585A JP 2020159585 A JP2020159585 A JP 2020159585A JP 6903804 B1 JP6903804 B1 JP 6903804B1
Authority
JP
Japan
Prior art keywords
layer
adhesive
window
image display
layers
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
JP2020159585A
Other languages
Japanese (ja)
Other versions
JP2021107913A (en
Inventor
康隆 石原
康隆 石原
孝伸 矢野
孝伸 矢野
翔 寳田
翔 寳田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nitto Denko Corp
Original Assignee
Nitto Denko Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nitto Denko Corp filed Critical Nitto Denko Corp
Priority to PCT/JP2020/037606 priority Critical patent/WO2021131218A1/en
Priority to CN202080024732.8A priority patent/CN113632235B/en
Priority to KR1020217025545A priority patent/KR102401803B1/en
Priority to TW109135011A priority patent/TWI753601B/en
Priority to JP2021032138A priority patent/JP6903830B1/en
Application granted granted Critical
Publication of JP6903804B1 publication Critical patent/JP6903804B1/en
Publication of JP2021107913A publication Critical patent/JP2021107913A/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

【課題】フレキシブル画像表示装置を高温環境下で繰り返し屈曲させたときに構成部材間の高い接着性を確保する。【解決手段】表示装置1はウインドウ部材11と第1部材と第1積層体Lまたはタッチセンサ付パネル部材と複数層の粘着部材21,22,23とを具備する。第1積層体は第2部材と第3A部材との積層体である。第1積層体を備える場合、第1部材および第2部材の一方は光学フィルム他方は光学フィルムまたはタッチセンサ13であり、複数層の粘着部材は少なくとも3層を含む。タッチセンサ付パネル部材を備える場合、複数層の粘着部材は各部材間に配置される2層を含む。E0×T0>0.32(E0:ウインドウ部材の弾性率(GPa)、T0:ウインドウ部材の厚み(mm))である。粘着部材の少なくとも1層の厚みは20μm以上であり、ウインドウ部材側からn番目の層および(n+1)番目の層の少なくとも一方の厚みは10μm以上である。【選択図】図1PROBLEM TO BE SOLVED: To secure high adhesiveness between constituent members when a flexible image display device is repeatedly bent in a high temperature environment. A display device 1 includes a window member 11, a first member, a first laminated body L, a panel member with a touch sensor, and a plurality of layers of adhesive members 21, 22, and 23. The first laminated body is a laminated body of the second member and the third A member. When the first laminated body is provided, one of the first member and the second member is an optical film, the other is an optical film or a touch sensor 13, and the plurality of layers of the adhesive member includes at least three layers. When the panel member with a touch sensor is provided, the plurality of layers of the adhesive member includes two layers arranged between the members. E0 × T0> 0.32 (E0: elastic modulus of the window member (GPa), T0: thickness of the window member (mm)). The thickness of at least one layer of the adhesive member is 20 μm or more, and the thickness of at least one of the nth layer and the (n + 1) th layer from the window member side is 10 μm or more. [Selection diagram] Fig. 1

Description

本発明は、複数層の粘着部材を備えるフレキシブル画像表示装置および光学積層体に関する。 The present invention relates to a flexible image display device and an optical laminate including a plurality of layers of adhesive members.

フレキシブル画像表示装置は、例えば、表示パネルを含むパネル部材と、パネル部材の前面に配置された光学積層体とを備える。光学積層体は、例えば、ウインドウ部材と、光学フィルムとを備えており、さらにタッチセンサを備える場合もある。光学積層体またはフレキシブル画像表示装置に含まれる各部材間には、接着層または粘着層が配置されている。 The flexible image display device includes, for example, a panel member including a display panel and an optical laminate arranged on the front surface of the panel member. The optical laminate includes, for example, a window member and an optical film, and may further include a touch sensor. An adhesive layer or an adhesive layer is arranged between each member included in the optical laminate or the flexible image display device.

例えば、特許文献1では、表示パネルと、表示パネル上に設けられた偏光部材と、偏光部材上に設けられたウインドーと、表示パネル及び偏光部材の間に設けられた第1接着部材と、偏光部材及びウインドーの間に設けられた第2接着部材とを含むフォルダブル表示装置が提案されている。特許文献1には、フォルダブル表示装置がタッチセンシングユニットを含むことができることが記載されている。また、特許文献1には、ウインドーWDと、タッチセンシングユニットTSUと、偏光部材POLと、表示パネルDPとを備えるフォルダブル表示装置が記載されている。ウインドーWDとタッチセンシングユニットTSUとの間には、第1接着部材AD1が配置され、タッチセンシングユニットTSUと偏光部材POLとの間には第4接着部材AD4が配置され、偏光部材POLと表示パネルDPとの間には第2接着部材AD2が配置されている。 For example, in Patent Document 1, a display panel, a polarizing member provided on the display panel, a window provided on the polarizing member, a first adhesive member provided between the display panel and the polarizing member, and polarization are provided. A foldable display device including a member and a second adhesive member provided between windows has been proposed. Patent Document 1 describes that a foldable display device can include a touch sensing unit. Further, Patent Document 1 describes a foldable display device including a window WD, a touch sensing unit TSU, a polarizing member POL, and a display panel DP. The first adhesive member AD1 is arranged between the window WD and the touch sensing unit TSU, and the fourth adhesive member AD4 is arranged between the touch sensing unit TSU and the polarizing member POL, and the polarizing member POL and the display panel. A second adhesive member AD2 is arranged between the DP and the DP.

特開2017−126061号公報(請求項1、[0132]、[0138]および図7B)JP-A-2017-126061 (Claim 1, [0132], [0138] and FIG. 7B)

フレキシブル画像表示装置は、装置を構成する部材(ウインドウ部材、光学フィルム、タッチセンサ、パネル部材など)を接着層または粘着層で貼り合わせた積層構造を有する。フレキシブル画像表示装置には、繰り返し屈曲させたときに、貼り合わせた部材間で剥離が生じない高い接着性が求められる。部材間の剥離は、高温環境下でフレキシブル画像表示装置を繰り返し屈曲させた場合には特に顕著になる。また、ウインドウ部材の硬さが高い(またはコシが強い)場合には、部材間の剥離が顕在化し易い。 The flexible image display device has a laminated structure in which members (window members, optical films, touch sensors, panel members, etc.) constituting the device are bonded together with an adhesive layer or an adhesive layer. The flexible image display device is required to have high adhesiveness that does not cause peeling between the bonded members when repeatedly bent. The peeling between the members becomes particularly remarkable when the flexible image display device is repeatedly bent in a high temperature environment. Further, when the hardness of the window member is high (or the stiffness is strong), peeling between the members is likely to become apparent.

本発明の一側面は、ウインドウ部材と、
前記ウインドウ部材に積層された第1部材と、
前記ウインドウ部材に前記第1部材を介して積層された第1積層体または第1タッチセンサ付パネル部材と、
複数層の粘着部材と、を具備するフレキシブル画像表示装置であって、
前記第1積層体は、前記ウインドウ部材に、前記第1部材を介して積層された第2部材と、前記第1部材および前記第2部材を介して積層された第3A部材との積層体であり、
前記フレキシブル画像表示装置が前記第1積層体を備える場合、
前記第1部材および前記第2部材の一方は、光学フィルムであり、他方は、光学フィルムまたはタッチセンサであり、
前記第3A部材は、少なくともパネル部材を含み、
前記複数層の粘着部材は、少なくとも、前記ウインドウ部材と前記第1部材との間、前記第1部材と前記第2部材との間、および前記第2部材と前記第3A部材との間に配置される3層を含み、
前記フレキシブル画像表示装置が前記第1タッチセンサ付パネル部材を備える場合、
前記第1部材は、光学フィルムであり、
前記複数層の粘着部材は、少なくとも、前記ウインドウ部材と前記第1部材との間、および前記第1部材と前記第1タッチセンサ付パネル部材との間に配置される2層を含み、
前記ウインドウ部材の弾性率(GPa)をE0とし、前記ウインドウ部材の厚み(mm)をT0とするとき、E0×T0(kN/mm)は、E0×T0>0.32の条件を満たし、
前記複数層の粘着部材の少なくとも1層の厚みは、20μm以上の条件を満たし、
前記複数層の粘着部材のうち、前記ウインドウ部材側からn番目の層および(n+1)番目の層の少なくとも一方の厚みは、10μm以上の条件を満たす、フレキシブル画像表示装置に関する。
One aspect of the present invention is a window member and
The first member laminated on the window member and
A first laminated body or a panel member with a first touch sensor laminated on the window member via the first member.
A flexible image display device including a plurality of layers of adhesive members.
The first laminated body is a laminated body of a second member laminated via the first member and a third A member laminated via the first member and the second member on the window member. Yes,
When the flexible image display device includes the first laminated body,
One of the first member and the second member is an optical film, and the other is an optical film or a touch sensor.
The third A member includes at least a panel member.
The plurality of layers of the adhesive member are arranged at least between the window member and the first member, between the first member and the second member, and between the second member and the third A member. Including 3 layers to be
When the flexible image display device includes the panel member with the first touch sensor,
The first member is an optical film and
The plurality of layers of the adhesive member includes at least two layers arranged between the window member and the first member and between the first member and the panel member with the first touch sensor.
When the elastic modulus (GPa) of the window member is E0 and the thickness (mm) of the window member is T0, E0 × T0 (kN / mm) satisfies the condition of E0 × T0> 0.32.
The thickness of at least one layer of the plurality of adhesive members satisfies the condition of 20 μm or more.
The present invention relates to a flexible image display device in which the thickness of at least one of the nth layer and the (n + 1) th layer from the window member side among the plurality of layers of the adhesive member satisfies a condition of 10 μm or more.

本発明の他の側面は、上記のフレキシブル画像表示装置に用いられ、
ウインドウ部材と、
前記ウインドウ部材に積層された第1部材と、
前記ウインドウ部材に前記第1部材を介して積層された第2積層体または第1セパレータと、
複数層の粘着部材と、を具備する光学積層体であって、
前記第2積層体は、前記ウインドウ部材に、前記第1部材を介して積層された第2部材と、前記第1部材および前記第2部材を介して積層された第3B部材との積層体であり、
前記光学積層体が前記第2積層体を備える場合、
前記第1部材および前記第2部材の一方は、光学フィルムであり、他方は、光学フィルムまたはタッチセンサであり、
前記第3B部材は、少なくとも第2セパレータを含み、
前記複数層の粘着部材は、少なくとも、前記ウインドウ部材と前記第1部材との間、前記第1部材と前記第2部材との間、および前記第2部材と前記第3B部材との間に配置される3層を含み、
前記光学積層体が前記第1セパレータを備える場合、
前記第1部材は、光学フィルムであり、
前記複数層の粘着部材は、少なくとも、前記ウインドウ部材と前記第1部材との間、および前記第1部材と前記第1セパレータとの間に配置される2層を含み、
前記ウインドウ部材の弾性率(GPa)をE0とし、前記ウインドウ部材の厚み(mm)をT0とするとき、E0×T0(kN/mm)は、E0×T0>0.32の条件を満たし、
前記複数層の粘着部材の少なくとも1層の厚みは、20μm以上の条件を満たし、
前記複数層の粘着部材のうち、前記ウインドウ部材側からn番目の層および(n+1)番目の層の少なくとも一方の厚みは、10μm以上の条件を満たす、光学積層体に関する。
Another aspect of the present invention is used in the flexible image display device described above.
Window members and
The first member laminated on the window member and
A second laminated body or a first separator laminated on the window member via the first member,
An optical laminate comprising a plurality of layers of adhesive members.
The second laminated body is a laminated body of a second member laminated via the first member and a third B member laminated via the first member and the second member on the window member. Yes,
When the optical laminate includes the second laminate,
One of the first member and the second member is an optical film, and the other is an optical film or a touch sensor.
The third B member includes at least a second separator.
The plurality of layers of the adhesive member are arranged at least between the window member and the first member, between the first member and the second member, and between the second member and the third B member. Including 3 layers to be
When the optical laminate includes the first separator
The first member is an optical film and
The plurality of layers of the adhesive member includes at least two layers arranged between the window member and the first member and between the first member and the first separator.
When the elastic modulus (GPa) of the window member is E0 and the thickness (mm) of the window member is T0, E0 × T0 (kN / mm) satisfies the condition of E0 × T0> 0.32.
The thickness of at least one layer of the plurality of adhesive members satisfies the condition of 20 μm or more.
The present invention relates to an optical laminate in which the thickness of at least one of the nth layer and the (n + 1) th layer from the window member side among the plurality of layers of the adhesive member satisfies the condition of 10 μm or more.

硬さが高いウインドウ部材を備えるフレキシブル画像表示装置を、高温環境下で繰り返し屈曲させたときに、積層した部材間の高い接着性を確保することができる。 When a flexible image display device provided with a window member having high hardness is repeatedly bent in a high temperature environment, high adhesiveness between the laminated members can be ensured.

本発明の第1実施形態に係るフレキシブル画像表示装置の概略断面図である。It is a schematic cross-sectional view of the flexible image display device which concerns on 1st Embodiment of this invention. 本発明の第2実施形態に係るフレキシブル画像表示装置の概略断面図である。It is the schematic sectional drawing of the flexible image display apparatus which concerns on 2nd Embodiment of this invention. 本発明の第3実施形態に係るフレキシブル画像表示装置の概略断面図である。It is the schematic sectional drawing of the flexible image display apparatus which concerns on 3rd Embodiment of this invention.

本発明に係るフレキシブル画像表示装置は、ウインドウ部材と、ウインドウ部材に積層された第1部材と、ウインドウ部材に第1部材を介して積層された第1積層体または第1タッチセンサ付パネル部材と、複数層の粘着部材と、を具備する。第1積層体は、ウインドウ部材に、第1部材を介して積層された第2部材と、第1部材および第2部材を介して積層された第3A部材との積層体である。 The flexible image display device according to the present invention includes a window member, a first member laminated on the window member, and a first laminated body or a panel member with a first touch sensor laminated on the window member via the first member. , With a plurality of layers of adhesive members. The first laminated body is a laminated body of a second member laminated via the first member and a third A member laminated via the first member and the second member on the window member.

フレキシブル画像表示装置が第1積層体を備える場合、第1部材および第2部材の一方は、光学フィルムであり、他方は、光学フィルムまたはタッチセンサである。第3A部材は、少なくともパネル部材を含む。この場合、複数層の粘着部材は、少なくとも、ウインドウ部材と第1部材との間、第1部材と第2部材との間、および第2部材と第3A部材との間に配置される3層を含む。 When the flexible image display device includes the first laminated body, one of the first member and the second member is an optical film, and the other is an optical film or a touch sensor. The third A member includes at least a panel member. In this case, the plurality of layers of the adhesive member are at least three layers arranged between the window member and the first member, between the first member and the second member, and between the second member and the third A member. including.

フレキシブル画像表示装置が第1タッチセンサ付パネル部材を備える場合、第1部材は、光学フィルムである。この場合、複数層の粘着部材は、少なくとも、ウインドウ部材と第1部材との間、および第1部材と第1タッチセンサ付パネル部材との間に配置される2層を含む。 When the flexible image display device includes a panel member with a first touch sensor, the first member is an optical film. In this case, the plurality of layers of the adhesive member includes at least two layers arranged between the window member and the first member and between the first member and the panel member with the first touch sensor.

また、本発明には、上記のフレキシブル画像表示装置に用いられる光学積層体も包含される。光学積層体は、ウインドウ部材と、ウインドウ部材に積層された第1部材と、ウインドウ部材に第1部材を介して積層された第2積層体または第1セパレータと、複数層の粘着部材と、を具備する。第2積層体は、ウインドウ部材に、第1部材を介して積層された第2部材と、第1部材および第2部材を介して積層された第3B部材との積層体である。 The present invention also includes an optical laminate used in the above-mentioned flexible image display device. The optical laminate includes a window member, a first member laminated on the window member, a second laminate or a first separator laminated on the window member via the first member, and a plurality of layers of adhesive members. Equipped. The second laminated body is a laminated body of a second member laminated via the first member and a third B member laminated via the first member and the second member on the window member.

光学積層体が第2積層体を備える場合、第1部材および第2部材の一方は、光学フィルムであり、他方は、光学フィルムまたはタッチセンサである。第3B部材は、少なくとも第2セパレータを含む。複数層の粘着部材は、少なくとも、ウインドウ部材と第1部材との間、第1部材と第2部材との間、および第2部材と第3B部材との間に配置される3層を含む。 When the optical laminated body includes the second laminated body, one of the first member and the second member is an optical film, and the other is an optical film or a touch sensor. The third B member includes at least a second separator. The multi-layer adhesive member includes at least three layers arranged between the window member and the first member, between the first member and the second member, and between the second member and the third B member.

光学積層体が第1セパレータを備える場合、第1部材は、光学フィルムである。この場合、複数層の粘着部材は、少なくとも、ウインドウ部材と第1部材との間、および第1部材と第1セパレータとの間に配置される2層を含む。 When the optical laminate includes a first separator, the first member is an optical film. In this case, the plurality of layers of the adhesive member includes at least two layers arranged between the window member and the first member and between the first member and the first separator.

光学積層体は、セパレータ(具体的には、第1セパレータまたは第3B部材に含まれる第2セパレータ)を剥離した状態でフレキシブル画像表示装置に用いられる。上記のフレキシブル画像表示装置は、セパレータを剥離した状態の光学積層体をウインドウ部材が視認側に配置された状態で含むことになる。 The optical laminate is used in a flexible image display device in a state where the separator (specifically, the first separator or the second separator included in the third B member) is peeled off. The flexible image display device includes an optical laminate with the separator peeled off, with the window member arranged on the viewing side.

上記のフレキシブル画像表示装置および光学積層体において、ウインドウ部材の弾性率(GPa)をE0とし、ウインドウ部材の厚み(mm)をT0とするとき、E0×T0(kN/mm)は、E0×T0>0.32の条件を満たす。弾性率と厚みとの積(=E0×T0)は、ウインドウ部材のコシ(または硬さ)の程度を示す。 In the above flexible image display device and optical laminate, when the elastic modulus (GPa) of the window member is E0 and the thickness (mm) of the window member is T0, E0 × T0 (kN / mm) is E0 × T0. The condition of> 0.32 is satisfied. The product (= E0 × T0) of the elastic modulus and the thickness indicates the degree of stiffness (or hardness) of the window member.

フレキシブル画像表示装置には、繰り返し屈曲させたときに、積層された構成部材間で剥離しない、高い接着性が求められる。構成部材間に粘着部材を配置することで、フレキシブル画像表示装置を屈曲させたときの応力を粘着部材により、ある程度緩和することができる。粘着部材は、硬化により各部材間を接着する接着部材とは異なり、各部材間を貼り合わせた状態でも高い粘性を備えるためである。 The flexible image display device is required to have high adhesiveness that does not peel off between the laminated constituent members when repeatedly bent. By arranging the adhesive member between the constituent members, the stress when the flexible image display device is bent can be relaxed to some extent by the adhesive member. This is because the adhesive member has a high viscosity even when the members are bonded to each other, unlike the adhesive member that adheres the members to each other by curing.

なお、接着部材は、硬化した接着剤であり、流動性を有さないものである。一方、粘着部材は、非硬化性の接着剤であり、流動性を有する。 The adhesive member is a cured adhesive and has no fluidity. On the other hand, the adhesive member is a non-curable adhesive and has fluidity.

フレキシブル画像表示装置の視認側に配置されるウインドウ部材の硬さが低い(またはコシが弱い)場合(具体的には、E0×T0≦0.32(kN/mm)の場合)には、粘着部材をフレキシブル画像表示装置内に複数層配置することで屈曲による応力を緩和できる。しかし、ウインドウ部材の硬さが高い(またはコシが強い)場合(具体的には、E0×T0>0.32(kN/mm)の場合)、粘着部材を複数層配置しても、屈曲による応力が十分に緩和されないことがあることが明らかとなった。また、フレキシブル画像表示装置を、室温(20℃〜35℃)で繰り返し屈曲させたときには、積層された部材間で剥離が生じない場合でも、高温環境下(例えば、60℃)で繰り返し屈曲させると剥離が生じて、高い接着性を確保できなくなる場合がある。 Adhesion when the hardness (or weakness) of the window member arranged on the visual side of the flexible image display device is low (specifically, when E0 × T0 ≦ 0.32 (kN / mm)) By arranging the members in a plurality of layers in the flexible image display device, the stress due to bending can be relaxed. However, when the hardness of the window member is high (or the stiffness is strong) (specifically, when E0 × T0> 0.32 (kN / mm)), even if a plurality of layers of the adhesive member are arranged, it is bent. It became clear that the stress may not be sufficiently relieved. Further, when the flexible image display device is repeatedly bent at room temperature (20 ° C. to 35 ° C.), even if peeling does not occur between the laminated members, the flexible image display device is repeatedly bent in a high temperature environment (for example, 60 ° C.). Peeling may occur, making it impossible to ensure high adhesiveness.

厚みが10μm未満(中でも、8μm以下、7μm以下、または6μm以下)の粘着部材の層は、屈曲による応力を緩和する効果が低い。特に、E0×T0>0.32(kN/mm)の場合、ウインドウ部材側からn番目および(n+1)番目の粘着部材の層の厚みが、連続して10μm未満であると、20μm以上の厚みを有する粘着部材の層を設けても、屈曲による応力を緩和することが難しい。本発明に係るフレキシブル画像表示装置および光学積層体では、少なくとも3層または少なくとも2層の粘着部材を設けるとともに、少なくとも1層の粘着部材の厚みを、20μm以上に制御する。加えて、複数層の粘着部材のうち、ウインドウ部材側からn番目の層および(n+1)番目の層の少なくとも一方の厚みを、10μm以上に制御する。少なくとも3層または少なくとも2層の粘着部材を設けることで、積層構造全体としての柔軟性が高まる。さらに、上記のように粘着部材の層の厚みを制御することで、E0×T0>0.32(kN/mm)の場合でも屈曲による応力を積層構造全体により効果的に緩和することができる。よって、フレキシブル画像表示装置を高温環境下で繰り返し屈曲させても、積層された部材間の剥離が効果的に抑制され、高い接着性を確保することができる。 A layer of an adhesive member having a thickness of less than 10 μm (especially, 8 μm or less, 7 μm or less, or 6 μm or less) has a low effect of relieving stress due to bending. In particular, in the case of E0 × T0> 0.32 (kN / mm), if the thickness of the nth and (n + 1) th adhesive member layers from the window member side is continuously less than 10 μm, the thickness is 20 μm or more. It is difficult to relieve the stress due to bending even if the layer of the adhesive member having In the flexible image display device and the optical laminate according to the present invention, at least three layers or at least two layers of adhesive members are provided, and the thickness of at least one layer of the adhesive members is controlled to 20 μm or more. In addition, the thickness of at least one of the nth layer and the (n + 1) th layer from the window member side among the plurality of layers of the adhesive member is controlled to be 10 μm or more. By providing at least three layers or at least two layers of adhesive members, the flexibility of the laminated structure as a whole is increased. Further, by controlling the thickness of the layer of the adhesive member as described above, the stress due to bending can be effectively relaxed by the entire laminated structure even when E0 × T0> 0.32 (kN / mm). Therefore, even if the flexible image display device is repeatedly bent in a high temperature environment, peeling between the laminated members is effectively suppressed, and high adhesiveness can be ensured.

なお、ウインドウ部材を始めとする、フレキシブル画像表示装置または光学積層体における各部材の硬さは、例えば、各部材の材質、層構成、および/または厚みを調節することにより調節できる。 The hardness of each member in the flexible image display device or the optical laminate including the window member can be adjusted by, for example, adjusting the material, layer structure, and / or thickness of each member.

(粘着部材)
光学積層体またはフレキシブル画像表示装置は、複数層の粘着部材を備えている。より具体的には、フレキシブル画像表示装置(または光学積層体)が第1積層体(または第2積層体)を備える場合、フレキシブル画像表示装置(または光学積層体)は、少なくとも、ウインドウ部材と第1部材との間、第1部材と第2部材との間、および第2部材と第3A部材(または第3B部材)との間に配置される3層の粘着部材を備える。フレキシブル画像表示装置(または光学積層体)が第1タッチセンサ付パネル部材(または第1セパレータ)を備える場合、複数層の粘着部材は、少なくとも、ウインドウ部材と第1部材との間、および第1部材と第1タッチセンサ付パネル部材(または第1セパレータ)との間に配置される2層の粘着部材を備える。複数層の粘着部材は、このような隣接する部材間に配される3層または2層の粘着部材以外の粘着部材を含んでもよい。上記3層または2層の粘着部材以外の粘着部材は、ウインドウ部材以外の各部材内(具体的には、第1部材、第2部材、第3A部材(または第3B部材)、および第1タッチセンサ付パネル部材からなる群より選択される少なくとも1つの部材内)に配置されている。各粘着部材は、通常、層状である。各部材内における粘着部材の個数は特に制限されず、0層であってもよく、1層であってもよく、2層以上であってもよい。このように、フレキシブル画像表示装置または光学積層体に含まれる粘着部材(つまり、複数層の粘着部材)には、隣接する各部材間に含まれる粘着部材および各部材内に含まれる粘着部材の双方が包含される。
(Adhesive member)
The optical laminate or the flexible image display device includes a plurality of layers of adhesive members. More specifically, when the flexible image display device (or optical laminate) includes the first laminate (or the second laminate), the flexible image display device (or the optical laminate) is at least the window member and the first. A three-layer adhesive member is provided between the first member, between the first member and the second member, and between the second member and the third A member (or the third B member). When the flexible image display device (or optical laminate) includes the panel member with the first touch sensor (or the first separator), the multi-layer adhesive member is at least between the window member and the first member, and the first. It includes a two-layer adhesive member arranged between the member and the panel member with the first touch sensor (or the first separator). The multi-layer adhesive member may include an adhesive member other than the three-layer or two-layer adhesive member arranged between such adjacent members. The adhesive member other than the three-layer or two-layer adhesive member is inside each member other than the window member (specifically, the first member, the second member, the third A member (or the third B member), and the first touch. It is arranged in at least one member selected from the group consisting of panel members with sensors). Each adhesive member is usually layered. The number of adhesive members in each member is not particularly limited, and may be 0 layer, 1 layer, or 2 or more layers. As described above, the adhesive member (that is, the adhesive member having a plurality of layers) included in the flexible image display device or the optical laminate includes both the adhesive member included between the adjacent members and the adhesive member contained in each member. Is included.

フレキシブル画像表示装置または光学積層体に含まれる粘着部材は、例えば、8層以下であってもよく、7層または6層以下であってもよく、5層または4層以下であってもよい。 The adhesive member included in the flexible image display device or the optical laminate may be, for example, 8 layers or less, 7 layers or 6 layers or less, or 5 layers or 4 layers or less.

複数層の粘着部材のうち、厚みが20μm以上である層は、少なくとも1層であり、2層以上であってもよい。厚みが20μm以上の粘着部材の層を設けることで、E0×T0>0.32(kN/mm)の場合でも、高温環境下でフレキシブル画像表示装置を繰り返し屈曲させたときの積層された部材間における高い接着性を確保することができる。 Among the plurality of layers of the adhesive member, the layer having a thickness of 20 μm or more is at least one layer, and may be two or more layers. By providing a layer of adhesive members with a thickness of 20 μm or more, even when E0 × T0> 0.32 (kN / mm), between the laminated members when the flexible image display device is repeatedly bent in a high temperature environment. High adhesiveness can be ensured.

複数層の粘着部材の厚みの最大値は、例えば、50μm以下であり、40μm以下であってもよい。フレキシブル画像表示装置は、視認側において、ウインドウ部材の表面が露出した状態で用いられる。そのため、フレキシブル画像表示装置の視認側の表面の耐傷性は、高いことが好ましい。フレキシブル画像表示装置に複数層の粘着部材が含まれる場合または粘着部材の層の厚みが大きい場合には、屈曲による応力を比較的緩和し易い。しかし、粘着部材が変形することで押圧痕が元に戻りにくくなるため、耐傷性は低下する。なお、硬化した接着部材の場合には、粘着部材の場合のような応力の緩和は起こり難く、耐傷性の低下はほとんど見られない。フレキシブル画像表示装置では、構成部材に高い柔軟性が求められるため、粘性の大きい粘着部材による耐傷性への影響が顕在化し易いと考えられる。本発明では、E0×T0>0.32(kN/mm)とするため、ある程度の耐傷性を確保できる。より高い耐傷性を確保し易い観点からは、複数層の粘着部材の厚みの最大値は、30μm以下が好ましく、27μm以下としてもよい。なお、表面の耐傷性は、例えば、鉛筆硬度試験により評価することができる。 The maximum thickness of the plurality of layers of the adhesive member is, for example, 50 μm or less, and may be 40 μm or less. The flexible image display device is used in a state where the surface of the window member is exposed on the visual side. Therefore, it is preferable that the surface of the flexible image display device on the visual side has high scratch resistance. When the flexible image display device includes a plurality of layers of adhesive members or when the layers of the adhesive members are thick, it is relatively easy to relieve stress due to bending. However, since the pressure marks are hard to return to the original due to the deformation of the adhesive member, the scratch resistance is lowered. In the case of a hardened adhesive member, it is difficult for stress to be relaxed as in the case of an adhesive member, and there is almost no decrease in scratch resistance. In a flexible image display device, since the constituent members are required to have high flexibility, it is considered that the influence of the highly viscous adhesive member on the scratch resistance is likely to become apparent. In the present invention, since E0 × T0> 0.32 (kN / mm), a certain degree of scratch resistance can be ensured. From the viewpoint of easily ensuring higher scratch resistance, the maximum thickness of the plurality of layers of the adhesive member is preferably 30 μm or less, and may be 27 μm or less. The scratch resistance of the surface can be evaluated by, for example, a pencil hardness test.

フレキシブル画像表示装置における耐傷性は、視認側の表面(より具体的には、ウインドウ部材の視認側の表面)について測定される。そのため、ウインドウ部材から離れた位置にある粘着部材の層よりも、ウインドウ部材と隣接する(つまり、ウインドウ部材側から1番目の)粘着部材の層の応力緩和性が耐傷性に影響し易い。また、E0×T0>0.32(kN/mm)の場合、E0×T0≦0.32(kN/mm)の場合に比べて、フレキシブル画像表示装置の視認側の表面を押圧したときの応力は、フレキシブル画像表示装置の積層構造全体で緩和される傾向がある。そのため、より高い耐傷性を確保する観点からは、ウインドウ部材側から1番目の粘着部材の層の厚みおよび複数層の粘着部材の厚みの平均値を制御することが好ましい。 The scratch resistance of the flexible image display device is measured with respect to the surface on the viewing side (more specifically, the surface on the viewing side of the window member). Therefore, the stress relaxation property of the layer of the adhesive member adjacent to the window member (that is, the first layer from the window member side) is more likely to affect the scratch resistance than the layer of the adhesive member located at a position away from the window member. Further, when E0 × T0> 0.32 (kN / mm), the stress when the surface on the visual side of the flexible image display device is pressed is compared with the case of E0 × T0 ≦ 0.32 (kN / mm). Tends to be relaxed throughout the laminated structure of the flexible image display device. Therefore, from the viewpoint of ensuring higher scratch resistance, it is preferable to control the average value of the layer thickness of the first adhesive member from the window member side and the thickness of the plurality of adhesive members.

より具体的には、フレキシブル画像表示装置または光学積層体に含まれる複数層の粘着部材の厚みの平均値は、例えば、23μm以下であり、より高い耐傷性を確保する観点からは、20μm以下が好ましく、20μm未満または19μm以下としてもよく、18μm以下としてもよい。 More specifically, the average value of the thicknesses of the plurality of layers of adhesive members contained in the flexible image display device or the optical laminate is, for example, 23 μm or less, and from the viewpoint of ensuring higher scratch resistance, 20 μm or less is used. Preferably, it may be less than 20 μm or 19 μm or less, or 18 μm or less.

ウインドウ部材側から1番目の粘着部材の層の厚みは、20μm以下が好ましく、20μm未満または17μm以下としてもよく、16μm以下または15μm以下としてもよい。 The thickness of the layer of the first adhesive member from the window member side is preferably 20 μm or less, may be less than 20 μm or 17 μm or less, and may be 16 μm or less or 15 μm or less.

換言すれば、より高い鉛筆硬度を確保する観点からは、厚みが20μmより大きい粘着部材の層は、ウインドウ部材側から2番目以降の位置に設けることが好ましい。 In other words, from the viewpoint of ensuring higher pencil hardness, it is preferable that the layer of the adhesive member having a thickness of more than 20 μm is provided at the second and subsequent positions from the window member side.

より高い接着性を確保する観点からは、フレキシブル画像表示装置を屈曲させた状態で内側に位置する粘着部材の層よりも、より外側に位置する粘着部材の層の厚みを20μm以上とすることが有利である。従って、このような観点からは、ウインドウ部材側から2番目以降の粘着部材の層の厚みを20μm以上とすることが好ましい。 From the viewpoint of ensuring higher adhesiveness, the thickness of the layer of the adhesive member located on the outer side of the layer of the adhesive member located on the inner side in the bent state of the flexible image display device may be 20 μm or more. It is advantageous. Therefore, from such a viewpoint, it is preferable that the thickness of the second and subsequent layers of the adhesive member from the window member side is 20 μm or more.

粘着部材の各層の厚みは、それぞれ、例えば、3μm以上であり、5μm以上または6μm以上であってもよい。粘着部材の層の厚みがこのような範囲である場合、フレキシブル画像表示装置における高い屈曲性を確保し易い。 The thickness of each layer of the adhesive member is, for example, 3 μm or more, and may be 5 μm or more or 6 μm or more. When the thickness of the layer of the adhesive member is within such a range, it is easy to secure high flexibility in the flexible image display device.

複数層の粘着部材のうち、ウインドウ部材側からn番目の層および(n+1)番目の層の少なくとも一方の厚みが、10μm以上であればよく、11μm以上または12μm以上であってもよく、14μm以上または15μm以上であってもよい。n番目の層および(n+1)番目の層の一方の厚みが10μm未満(好ましくは8μm以下、より好ましくは7μm以下または6μm以下)の場合、より高い接着性を確保する観点からは、他方の厚みは、14μm以上または15μm以上が好ましい。 Of the plurality of layers of the adhesive member, at least one of the nth layer and the (n + 1) th layer from the window member side may have a thickness of 10 μm or more, 11 μm or more, 12 μm or more, and 14 μm or more. Alternatively, it may be 15 μm or more. When the thickness of one of the nth layer and the (n + 1) th layer is less than 10 μm (preferably 8 μm or less, more preferably 7 μm or less or 6 μm or less), the thickness of the other layer is ensured from the viewpoint of ensuring higher adhesiveness. Is preferably 14 μm or more or 15 μm or more.

なお、フレキシブル画像表示装置では、ウインドウ部材の第1部材側の表面とタッチセンサまたはタッチセンサ付パネル部材(具体的には、第1または第2タッチセンサ付パネル部材)との間において、少なくとも1層の粘着部材と接触するように、加飾層が設けられることがある。加飾層を設ける部分の粘着部材の厚みが小さいと、加飾層により形成される段差を粘着部材で吸収し難くなる。そのため、加飾層による段差を吸収し易い観点から、加飾層が接触する粘着部材の厚みを10μm以上としてもよい。 In the flexible image display device, at least 1 is provided between the surface of the window member on the first member side and the touch sensor or the panel member with the touch sensor (specifically, the panel member with the first or second touch sensor). A decorative layer may be provided so as to come into contact with the adhesive member of the layer. If the thickness of the adhesive member at the portion where the decorative layer is provided is small, it becomes difficult for the adhesive member to absorb the step formed by the decorative layer. Therefore, from the viewpoint of easily absorbing the step caused by the decorative layer, the thickness of the adhesive member with which the decorative layer comes into contact may be 10 μm or more.

加飾層による段差を吸収し易い観点から、加飾層が接触する粘着部材の厚みを、加飾層の厚みの1.5倍以上としてもよく、2倍以上または2.5倍以上、さらには3倍以上としてもよい。 From the viewpoint of easily absorbing the step caused by the decorative layer, the thickness of the adhesive member with which the decorative layer comes into contact may be 1.5 times or more the thickness of the decorative layer, or 2 times or more or 2.5 times or more, and further. May be tripled or more.

上述した粘着部材の層の厚みの上限値と下限値とは任意に組み合わせることができる。 The upper limit value and the lower limit value of the layer thickness of the adhesive member described above can be arbitrarily combined.

粘着部材の各層の厚みは、フレキシブル画像表示装置または光学積層体の断面を切り出し、当該断面の走査型電子顕微鏡(SEM)による画像に基づいて測定される。粘着部材の各層の厚みは、上記断面のSEM画像において、加飾層が形成されていない部分について任意の複数箇所(例えば、5箇所)で厚みを測定し、平均化することにより求められる。 The thickness of each layer of the adhesive member is measured based on a cross section of a flexible image display device or an optical laminate cut out and an image of the cross section taken by a scanning electron microscope (SEM). The thickness of each layer of the adhesive member is obtained by measuring and averaging the thicknesses of the portions where the decorative layer is not formed at an arbitrary plurality of locations (for example, 5 locations) in the SEM image of the cross section.

粘着部材の各層の25℃における貯蔵弾性率は、通常、10MPa以下であり、3MPa以下または2MPa以下であってもよく、1.5MPa以下であってもよい。各粘着部材の25℃における貯蔵弾性率は、好ましくは1MPa以下であり、0.3MPa以下または0.2MPa以下であってもよく、0.15MPa以下または0.1MPa以下であってもよい。粘着部材の各層の貯蔵弾性率がこのような範囲である場合、高い接着性を確保できる。一方で、粘着部材の層の貯蔵弾性率が上記の範囲である場合、硬化した接着部材の場合とは異なり、押圧による応力を緩和し易く、鉛筆硬度が低下し易い。フレキシブル画像表示装置が、このように押圧による応力を緩和し易い粘着部材を複数層含む場合でも、E0×T0>0.32(kN/mm)とすることで、ある程度高い鉛筆硬度を確保することができる。また、ウインドウ部材側から1番目の粘着部材の層の厚みおよび複数層の粘着部材の平均厚みを上述のように制御することで、より高い鉛筆硬度を確保することもできる。 The storage elastic modulus of each layer of the adhesive member at 25 ° C. is usually 10 MPa or less, may be 3 MPa or less, 2 MPa or less, or 1.5 MPa or less . The storage elastic modulus of each adhesive member at 25 ° C. is preferably 1 MPa or less, 0.3 MPa or less or 0.2 MPa or less, and 0.15 MPa or less or 0.1 MPa or less. When the storage elastic modulus of each layer of the adhesive member is in such a range, high adhesiveness can be ensured. On the other hand, when the storage elastic modulus of the layer of the adhesive member is in the above range, unlike the case of the cured adhesive member, the stress due to pressing is easily relieved and the pencil hardness is easily lowered. Even when the flexible image display device includes a plurality of layers of adhesive members that can easily relieve stress due to pressing, a certain high pencil hardness can be ensured by setting E0 × T0> 0.32 (kN / mm). Can be done. Further, by controlling the thickness of the layer of the first adhesive member from the window member side and the average thickness of the plurality of adhesive members as described above, it is possible to secure a higher pencil hardness.

粘着部材の各層の25℃における貯蔵弾性率は、0.001MPa以上であってもよく、0.005MPa以上であってもよい。 The storage elastic modulus of each layer of the adhesive member at 25 ° C. may be 0.001 MPa or more, or 0.005 MPa or more.

上述した粘着部材の各層の貯蔵弾性率の上限値と下限値とは任意に組み合わせることができる。 The upper limit value and the lower limit value of the storage elastic modulus of each layer of the adhesive member described above can be arbitrarily combined.

一方、接着部材の25℃における貯蔵弾性率は、10MPaより大きく、100MPa以上であってもよく、通常、1GPa程度である。本明細書中、接着部材とは、このような貯蔵弾性率を有するものを意味するものとする。
このように、粘着部材は、接着部材とは貯蔵弾性率により区別される。
On the other hand, the storage elastic modulus of the adhesive member at 25 ° C. is larger than 10 MPa, may be 100 MPa or more, and is usually about 1 GPa. In the present specification, the adhesive member means a member having such a storage elastic modulus.
In this way, the adhesive member is distinguished from the adhesive member by the storage elastic modulus.

粘着部材の貯蔵弾性率は、JIS K 7244−1:1998に準拠して測定できる。具体的には、まず、粘着部材を用いて、厚み約1.5mmの成形物を作製する。この成形物を直径7.9mmの円盤状に打ち抜いて、試験片を作製する。この試験片を、パラレルプレートに挟み込み、動的粘弾測定装置(例えば、Rheometric Scientific社製「Advanced Rheometric Expansion System(ARES)」)を用いて、下記の条件で粘弾性の測定を行い、25℃における貯蔵弾性率を求める。なお、接着部材の貯蔵弾性率も、粘着部材の場合に準じて求められる。 The storage elastic modulus of the adhesive member can be measured according to JIS K 7244-1: 1998. Specifically, first, a molded product having a thickness of about 1.5 mm is produced using an adhesive member. This molded product is punched into a disk shape having a diameter of 7.9 mm to prepare a test piece. This test piece is sandwiched between parallel plates, and the viscoelasticity is measured under the following conditions using a dynamic viscoelasticity measuring device (for example, "Advanced Rheometric Expansion System (ARES)" manufactured by Rheometric Scientific), and the viscoelasticity is measured at 25 ° C. The storage elastic modulus in. The storage elastic modulus of the adhesive member is also obtained in the same manner as in the case of the adhesive member.

(測定条件)
変形モード:ねじり
測定周波数:1Hz
測定温度:−40℃〜+150℃
昇温度:5℃/分
(Measurement condition)
Deformation mode: Torsion measurement frequency: 1Hz
Measurement temperature: -40 ° C to + 150 ° C
Heating speed: 5 ° C. / min

本発明に係るフレキシブル画像表示装置では、視認側の表面(より具体的には、ウインドウ部材の視認側の表面)の鉛筆硬度がH以上の、高い鉛筆硬度を確保することができる。また、本発明に係るフレキシブル画像表示装置では、ウインドウ部材側において、3H以上または4H以上の高い鉛筆硬度を確保することもできる。 In the flexible image display device according to the present invention, it is possible to secure a high pencil hardness such that the pencil hardness of the surface on the viewing side (more specifically, the surface on the viewing side of the window member) is H or more. Further, in the flexible image display device according to the present invention, it is possible to secure a high pencil hardness of 3H or more or 4H or more on the window member side.

なお、本明細書中、鉛筆硬度は、JIS K 5600−5−4:1999に規定されるひっかき硬度(鉛筆法)を意味する。鉛筆硬度は、JIS K 5600−5−4:1999に準拠して、荷重750g重、25℃の条件下で測定することができる。 In this specification, the pencil hardness means the scratch hardness (pencil method) defined in JIS K 5600-5-4: 1999. Pencil hardness can be measured under the conditions of a load of 750 g and a weight of 25 ° C. in accordance with JIS K 5600-5-4: 1999.

パネル部材の高い視認性を確保する観点から、各粘着部材の全光線透過率は、85%以上が好ましく、90%以上がより好ましい。 From the viewpoint of ensuring high visibility of the panel members, the total light transmittance of each adhesive member is preferably 85% or more, more preferably 90% or more.

粘着部材の全光線透過率はJIS K 7136K:2000に準拠して測定できる。測定には、無アルカリガラス(厚さ0.8〜1.0mm、全光線透過率92%)に、粘着部材を約1.5mmの厚みになるまで配した試験片が用いられる。 The total light transmittance of the adhesive member can be measured according to JIS K 7136K: 2000. For the measurement, a test piece in which an adhesive member is arranged on non-alkali glass (thickness 0.8 to 1.0 mm, total light transmittance 92%) until the thickness becomes about 1.5 mm is used.

各粘着部材は、粘着剤により構成される。粘着剤の種類は特に制限されず、例えば、アクリル系粘着剤、ゴム系粘着剤、シリコーン系粘着剤、ウレタン系粘着剤、ビニルアルキルエーテル系粘着剤、ポリビニルピロリドン系粘着剤、ポリアクリルアミド系粘着剤、およびセルロース系粘着剤などが挙げられる。粘着剤には、例えば、ベースポリマー、架橋剤、添加剤(例えば、粘着付与剤、カップリング剤、重合禁止剤、架橋遅延剤、触媒、可塑剤、軟化剤、充填剤、着色剤、金属粉、紫外線吸収剤、光安定剤、酸化防止剤、劣化防止剤、界面活性剤、帯電防止剤、表面潤滑剤、レベリング剤、腐食防止剤、無機または有機系材料の粒子(金属化合物粒子(金属酸化物粒子など)、樹脂粒子など))が含まれ得るが、これらに限定されるものではない。 Each adhesive member is composed of an adhesive. The type of adhesive is not particularly limited, and for example, acrylic adhesive, rubber adhesive, silicone adhesive, urethane adhesive, vinyl alkyl ether adhesive, polyvinylpyrrolidone adhesive, polyacrylamide adhesive. , And a cellulose-based pressure-sensitive adhesive. Adhesives include, for example, base polymers, cross-linking agents, additives (eg, tackifiers, coupling agents, polymerization inhibitors, cross-linking retarders, catalysts, plasticizers, softeners, fillers, colorants, metal powders. , Ultraviolet absorbers, light stabilizers, antioxidants, deterioration inhibitors, surfactants, antistatic agents, surface lubricants, leveling agents, corrosion inhibitors, particles of inorganic or organic materials (metal compound particles (metal oxidation) (Object particles, etc.), resin particles, etc.))) are included, but are not limited thereto.

粘着剤として、上記のような貯蔵弾性率が得られる粘着剤を用いると、粘着部材の厚みを制御することによる効果が顕著になり易いため有利である。複数層の粘着部材のうち、少なくとも2層の粘着部材を構成する粘着剤は同じであってもよく、各粘着部材を構成する粘着剤は異なるものであってもよい。 It is advantageous to use a pressure-sensitive adhesive having the above-mentioned storage elastic modulus as the pressure-sensitive adhesive because the effect of controlling the thickness of the pressure-sensitive adhesive member tends to be remarkable. Of the plurality of layers of the pressure-sensitive adhesive member, the pressure-sensitive adhesives constituting at least two layers of the pressure-sensitive adhesive members may be the same, and the pressure-sensitive adhesives constituting each pressure-sensitive adhesive member may be different.

粘着部材は、例えば、各粘着部材を挟持させる部材の一方に、各粘着部材を構成する粘着剤を塗布したり、シート状に成形された粘着剤を転写したりすることにより形成できる。そして、各粘着部材を挟持させる部材の他方を粘着部材に積層することにより、各粘着部材が各部材間に配置される。粘着部材が各部材内に含まれる場合にも、各部材間に配置される場合に準じて粘着部材が各部材内に配置される。例えば、各部材を構成し、かつ粘着部材を挟持させる層(または積層体)の一方に、上記のような粘着剤の塗布または転写を利用して粘着部材を配置し、他方の層(または積層体)を粘着部材に貼り付けることにより粘着部材が各部材内に配置される。 The pressure-sensitive adhesive member can be formed, for example, by applying a pressure-sensitive adhesive constituting each pressure-sensitive adhesive member to one of the members that sandwich each pressure-sensitive adhesive member, or by transferring a pressure-sensitive adhesive molded into a sheet shape. Then, by laminating the other of the members that sandwich each adhesive member on the adhesive member, each adhesive member is arranged between the members. Even when the adhesive member is included in each member, the adhesive member is arranged in each member in the same manner as when the adhesive member is arranged between the members. For example, the adhesive member is arranged on one of the layers (or laminates) constituting each member and sandwiching the adhesive member by utilizing the application or transfer of the adhesive as described above, and the other layer (or laminate) is arranged. The adhesive member is arranged in each member by attaching the body) to the adhesive member.

(ウインドウ部材)
ウインドウ部材は、光学フィルム、タッチセンサ、タッチセンサ付パネル部材、およびパネル部材の破損防止のために、フレキシブル画像表示装置または光学積層体の視認側の最表面に配置される。
(Window member)
The window member is arranged on the outermost surface of the flexible image display device or the optical laminate on the visual side in order to prevent damage to the optical film, the touch sensor, the panel member with the touch sensor, and the panel member.

ウインドウ部材の弾性率E0と厚みT0との積がE0×T0>0.32(kN/mm)である場合、フレキシブル画像表示装置を高温環境下において繰り返し屈曲させたときの積層された部材間(または各部材を構成する層間)における接着性が低下し易い。本発明では、複数層の粘着部材の厚みを上記のように制御することで、E0×T0>0.32(kN/mm)の場合であっても、高温環境下でも高い接着性を確保することができる。 When the product of the elastic modulus E0 of the window member and the thickness T0 is E0 × T0> 0.32 (kN / mm), the space between the laminated members when the flexible image display device is repeatedly bent in a high temperature environment ( Alternatively, the adhesiveness between the layers constituting each member) tends to decrease. In the present invention, by controlling the thickness of the plurality of layers of the adhesive member as described above, high adhesiveness is ensured even in a high temperature environment even when E0 × T0> 0.32 (kN / mm). be able to.

ウインドウ部材は、通常、ウインドウフィルムを備えている。フレキシブル画像表示装置またはこれに適用される光学積層体には、高い柔軟性(高可換性など)、高い透明性(高い全光線透過率および低いへイズなど)、および高い硬度が求められる。ウインドウフィルムの材質は、これらの物性を満たすものであれば特に制限されない。 The window member usually includes a window film. Flexible image display devices or optical laminates applied thereto are required to have high flexibility (high commutativity, etc.), high transparency (high total light transmittance, low haze, etc.), and high hardness. The material of the window film is not particularly limited as long as it satisfies these physical characteristics.

ウインドウフィルムとしては、例えば、透明樹脂フィルムが挙げられる。透明樹脂フィルムを構成する樹脂としては、例えば、ポリイミド系樹脂、ポリアミド系樹脂、ポリエステル系樹脂、セルロース系樹脂、アセテート系樹脂、スチレン系樹脂、スルホン系樹脂、エポキシ系樹脂、ポリオレフィン系樹脂、ポリエーテルエーテルケトン系樹脂、スルフィド系樹脂、ビニルアルコール系樹脂、ウレタン系樹脂、アクリル系樹脂、およびポリカーボネート系樹脂から選択される少なくとも一種が挙げられる。しかし、透明樹脂フィルムを構成する樹脂はこれらに限定されるものではない。 Examples of the window film include a transparent resin film. Examples of the resin constituting the transparent resin film include polyimide resin, polyamide resin, polyester resin, cellulose resin, acetate resin, styrene resin, sulfone resin, epoxy resin, polyolefin resin, and polyether. At least one selected from ether ketone resin, sulfide resin, vinyl alcohol resin, urethane resin, acrylic resin, and polycarbonate resin can be mentioned. However, the resin constituting the transparent resin film is not limited to these.

ウインドウフィルムの厚みは、例えば、20μm以上500μm以下であり、30μm以上200μm以下であってもよい。ウインドウフィルムがこのような厚みである場合、高い強度と高い屈曲性とを両立し易い。 The thickness of the window film is, for example, 20 μm or more and 500 μm or less, and may be 30 μm or more and 200 μm or less. When the window film has such a thickness, it is easy to achieve both high strength and high flexibility.

本明細書中、粘着部材以外の部材(成形体)または粘着剤以外の材料について、透明なものとは、試験片の全光線透過率が80%以上であるものを意味する。全光線透過率の測定には、透明な材料または部材で構成される厚みが約1.5mmの試験片が用いられる。全光線透過率は、粘着部材の場合に準じて測定できる。 In the present specification, with respect to a member (molded body) other than the adhesive member or a material other than the adhesive, the transparent material means that the total light transmittance of the test piece is 80% or more. A test piece having a thickness of about 1.5 mm and made of a transparent material or member is used for measuring the total light transmittance. The total light transmittance can be measured according to the case of the adhesive member.

ウインドウ部材は、ハードコート層を備えていてもよい。ウインドウフィルムの高い破損防止効果が得られ易い観点から、ハードコート層は、少なくともウインドウ部材の第1部材側とは反対側に設けられていることが好ましい。より具体的には、ハードコート層は、少なくともウインドウフィルムの第1部材側とは反対側(つまり、ウインドウフィルムの視認側)の表面に設けられていることが好ましい。 The window member may include a hard coat layer. From the viewpoint that a high damage prevention effect of the window film can be easily obtained, it is preferable that the hard coat layer is provided at least on the side opposite to the first member side of the window member. More specifically, it is preferable that the hard coat layer is provided on the surface at least on the side opposite to the first member side of the window film (that is, the visible side of the window film).

ハードコート層の厚みは、例えば、1μm以上100μm以下であり、1μm以上50μm以下であってもよい。ウインドウ部材が複数のハードコート層を備える場合、各ハードコート層の厚みをこのような範囲とすればよい。 The thickness of the hard coat layer is, for example, 1 μm or more and 100 μm or less, and may be 1 μm or more and 50 μm or less. When the window member includes a plurality of hard coat layers, the thickness of each hard coat layer may be within such a range.

ハードコート層は、例えば、硬化性のコーティング剤を下地となる層(例えば、ウインドウフィルム)の表面に塗布し、硬化させることにより形成される。 The hard coat layer is formed, for example, by applying a curable coating agent to the surface of a underlying layer (for example, a window film) and curing it.

コーティング剤としては、例えば、光学フィルム用途のものが利用できる。コーティング剤として、例えば、アクリル系コーティング剤、メラミン系コーティング剤、ウレタン系コーティング剤、エポキシ系コーティング剤、シリコーン系コーティング剤、無機系コーティング剤が挙げられるが、これらに限定されるものではない。 As the coating agent, for example, those used for optical films can be used. Examples of the coating agent include, but are not limited to, an acrylic coating agent, a melamine coating agent, a urethane coating agent, an epoxy coating agent, a silicone coating agent, and an inorganic coating agent.

コーティング剤は、添加剤を含んでもよい。添加剤としては、例えば、シランカップリング剤、着色剤、染料、粉体または粒子(顔料、無機または有機の充填剤、無機または有機系材料の粒子等)、界面活性剤、可塑剤、帯電防止剤、表面潤滑剤、レベリング剤、酸化防止剤、光安定剤、紫外線吸収剤、重合禁止剤、防汚材等が挙げられるが、これらに限定されるものではない。 The coating agent may contain additives. Additives include, for example, silane coupling agents, colorants, dyes, powders or particles (pigments, inorganic or organic fillers, particles of inorganic or organic materials, etc.), surfactants, plasticizers, antistatic agents. Examples thereof include, but are not limited to, agents, surface lubricants, leveling agents, antioxidants, light stabilizers, ultraviolet absorbers, polymerization inhibitors, antifouling materials, and the like.

ウインドウ部材は、必要に応じて、他の層(以下、層Aと称する。)を備えていてもよい。層Aとしては、反射防止層、防眩層、防汚層、スティッキング防止層、色相調整層、帯電防止層、易接着層、イオンまたはオリゴマー等の析出防止層、衝撃吸収層、飛散防止層などが挙げられる。ウインドウ部材は、層Aを1層含んでいてもよく、複数層含んでいてもよい。層Aは、例えば、ウインドウ部材を構成する他の層または積層体(例えば、ウインドウフィルム)の表面側もしくは第1部材側に設けられている。層Aは、ウインドウフィルムを構成する他の層または積層体上に、コーティングなどにより直接形成されていてもよく、接着部材を介して積層されていてもよい。なお、ウインドウ部材は、粘着部材を含まない。ここで粘着部材とは、上記のような25℃における貯蔵弾性率を備える粘着部材を言うものとする。 The window member may include another layer (hereinafter, referred to as layer A), if necessary. The layer A includes an antireflection layer, an antiglare layer, an antifouling layer, a sticking prevention layer, a hue adjustment layer, an antistatic layer, an easy-adhesion layer, a precipitation prevention layer such as ions or oligomers, a shock absorption layer, and a shatterproof layer. Can be mentioned. The window member may include one layer A or a plurality of layers. The layer A is provided, for example, on the surface side or the first member side of another layer or laminate (for example, a window film) constituting the window member. The layer A may be directly formed by a coating or the like on another layer or a laminated body constituting the window film, or may be laminated via an adhesive member. The window member does not include an adhesive member. Here, the adhesive member refers to an adhesive member having a storage elastic modulus at 25 ° C. as described above.

ウインドウ部材の厚みT0は、例えば、0.02mm以上0.3mm以下であり、0.04mm以上0.2mm以下であってもよい。 The thickness T0 of the window member is, for example, 0.02 mm or more and 0.3 mm or less, and may be 0.04 mm or more and 0.2 mm or less.

ウインドウ部材の厚みT0は、フレキシブル画像表示装置または光学積層体の断面を切り出し、当該断面のSEMによる画像に基づいて測定される。厚みT0は、上記断面のSEM画像において、任意の複数箇所(例えば、5箇所)で厚みを測定し、平均化することにより求められる。 The thickness T0 of the window member is measured based on a cross section of the flexible image display device or the optical laminate and an SEM image of the cross section. The thickness T0 is obtained by measuring the thickness at an arbitrary plurality of points (for example, 5 points) and averaging the thickness in the SEM image of the cross section.

なお、本明細書中、光学積層体またはフレキシブル画像表示装置を構成する部材の厚みは、ウインドウ部材の厚みT0の場合に準じて求められる。 In the present specification, the thickness of the member constituting the optical laminate or the flexible image display device is obtained according to the case of the thickness T0 of the window member.

ウインドウ部材の弾性率E0は、例えば、0.53GPa以上16GPa以下であり、0.6GPaより大きく16GPa未満、1GPa以上15GPa以下、1GPa以上10GPa以下、または3GPa以上8GPa以下であってもよい。 The elastic modulus E0 of the window member may be, for example, 0.53 GPa or more and 16 GPa or less, greater than 0.6 GPa and less than 16 GPa, 1 GPa or more and 15 GPa or less, 1 GPa or more and 10 GPa or less, or 3 GPa or more and 8 GPa or less.

ウインドウ部材の弾性率E0(GPa)は、ウインドウ部材の測定用サンプルを3つ準備し、各サンプルの弾性率を引張試験により測定し、平均化することにより得られる平均値(算術平均値)である。引張り試験は、下記の装置を用いて下記の条件で行うことができる。
引張試験機:(株)島津製作所製、オートグラフAG−1S
コントロール:ストローク
標点距離:100mm
引張速度:50mm/min
弾性率算出範囲:10N/mm〜20N/mm
The elastic modulus E0 (GPa) of the window member is an average value (arithmetic mean value) obtained by preparing three samples for measuring the window member, measuring the elastic modulus of each sample by a tensile test, and averaging them. is there. The tensile test can be performed under the following conditions using the following device.
Tensile tester: Shimadzu Corporation, Autograph AG-1S
Control: Stroke Station distance: 100 mm
Tensile rate: 50 mm / min
Elastic modulus calculation range: 10N / mm 2 to 20N / mm 2

なお、弾性率測定用のサンプルは、次のようにして作製される。まず、ウインドウ部材の縦および横の弾性率を測定する。次いで、ウインドウ部材を、弾性率が高い方向の長さを150mmとし、弾性率が低い方向の長さを10mmとして、短冊状にカットすることによりサンプルが作製される。ウインドウ部材のカットには、例えば、ダンベル社製の多目的試験片裁断機が用いられる。 The sample for measuring the elastic modulus is prepared as follows. First, the elastic modulus of the window member in the vertical and horizontal directions is measured. Next, a sample is prepared by cutting the window member into strips with a length in the direction of high elastic modulus of 150 mm and a length of 10 mm in the direction of low elastic modulus. For cutting the window member, for example, a multipurpose test piece cutting machine manufactured by Dumbbell Co., Ltd. is used.

E0×T0は、0.32kN/mmより大きければよく、0.33kN/mm以上であってもよく、0.34kN/mm以上または0.35kN/mm以上であってもよい。より高い屈曲性を確保し易い観点から、E0×T0は、例えば、1.5kN/mm以下であり、1.0kN/mm以下であってもよい。これらの下限値と上限値とは任意に組み合わせることができる。 E0 × T0 may be larger than 0.32 kN / mm, may be 0.33 kN / mm or more, and may be 0.34 kN / mm or more or 0.35 kN / mm or more. From the viewpoint of easily ensuring higher flexibility, E0 × T0 is, for example, 1.5 kN / mm or less, and may be 1.0 kN / mm or less. These lower limit values and upper limit values can be arbitrarily combined.

(第1部材および第2部材)
フレキシブル画像表示装置および光学積層体において、第1部材は、ウインドウ部材に積層されている。フレキシブル画像表示装置(または光学積層体)が第1積層体(または第2積層体)を備える場合、第2部材は、ウインドウ部材に第1部材を介して積層されている。ウインドウ部材と第1部材との間、および第1部材と第2部材との間には、それぞれ、粘着部材が介在した状態である。フレキシブル画像表示装置(または光学積層体)が第1積層体(または第2積層体)を備える場合、第1部材および第2部材の一方は光学フィルムであり、他方は光学フィルムまたはタッチセンサである。フレキシブル画像表示装置(または光学積層体)は、第3A部材(または第3B部材)を備え、第1部材および第2部材の一方は光学フィルムであり、他方はタッチセンサであってもよい。フレキシブル画像表示装置が第1タッチセンサ付パネル部材を備える場合および光学積層体が第1セパレータを備える場合、第1部材は光学フィルムであってもよい。また、第3A部材が第2タッチセンサ付パネル部材を含む場合、第1部材および第2部材のそれぞれは、光学フィルムであってもよい。
(1st member and 2nd member)
In the flexible image display device and the optical laminate, the first member is laminated on the window member. When the flexible image display device (or optical laminated body) includes the first laminated body (or the second laminated body), the second member is laminated on the window member via the first member. An adhesive member is interposed between the window member and the first member, and between the first member and the second member, respectively. When the flexible image display device (or optical laminate) includes the first laminate (or the second laminate), one of the first member and the second member is an optical film, and the other is an optical film or a touch sensor. .. The flexible image display device (or optical laminate) includes a third A member (or a third B member), one of the first member and the second member may be an optical film, and the other may be a touch sensor. When the flexible image display device includes the panel member with the first touch sensor and the optical laminate includes the first separator, the first member may be an optical film. When the third A member includes a panel member with a second touch sensor, each of the first member and the second member may be an optical film.

第1部材および第2部材は、フレキシブル画像表示装置に含まれる部材であるため、適度な強度および柔軟性を有する。第1部材および第2部材の弾性率(GPa)を、それぞれ、E1およびE2とし、第1部材および第2部材の厚み(mm)を、それぞれ、T1およびT2とする。このとき、第1部材および第2部材は、それぞれ、下記を充足することが好ましい。各部材において、弾性率と厚みとの積がこのような範囲であることで、粘着部材の各層の厚みを上述のように制御することによる効果がさらに得られ易くなる。
0.01(kN/mm)≦E1×T1≦0.35(kN/mm)(第1部材)
0.01(kN/mm)≦E2×T2≦0.35(kN/mm)(第2部材)
Since the first member and the second member are members included in the flexible image display device, they have appropriate strength and flexibility. The elastic moduli (GPa) of the first member and the second member are E1 and E2, respectively, and the thicknesses (mm) of the first member and the second member are T1 and T2, respectively. At this time, it is preferable that the first member and the second member each satisfy the following. When the product of the elastic modulus and the thickness of each member is in such a range, the effect of controlling the thickness of each layer of the adhesive member as described above can be further easily obtained.
0.01 (kN / mm) ≤ E1 x T1 ≤ 0.35 (kN / mm) (first member)
0.01 (kN / mm) ≤ E2 x T2 ≤ 0.35 (kN / mm) (second member)

(光学フィルム)
光学フィルムとは、光学的機能を付与するフィルムである。光学フィルムは、通常、光学的機能を有する少なくとも1つの層を含む積層体である。光学フィルムとしては、画像表示装置の分野などで利用されるものが挙げられる。第1部材および第2部材のそれぞれは、光学フィルムであってもよく、または光学フィルムを構成する1つの層もしくは2つ以上の層の積層体であってもよい。
(Optical film)
The optical film is a film that imparts an optical function. An optical film is usually a laminate containing at least one layer having an optical function. Examples of the optical film include those used in the field of image display devices and the like. Each of the first member and the second member may be an optical film, or may be one layer or a laminate of two or more layers constituting the optical film.

光学的機能を有する層としては、例えば、光学異方性を有する層(例えば、光学異方性フィルム)が挙げられる。光学異方性を有する層としては、例えば、偏光子、位相差層、視野角拡大フィルム、視野角制限(覗き見止)フィルム、輝度向上フィルム、光学補償フィルムが挙げられるが、これらに限定されるものではない。2つ以上の層の積層体は、これらの光学異方性を有する層から選択される2つ以上を有するものであってもよい。2つ以上の層の積層体において、光学異方性を有する層の全てが異なる機能を有するものであってもよく、少なくとも2つの層が同じ機能を有するものであってもよい。例えば、積層体は、偏光子と位相差層とを含んでいてもよく、組成の異なる2つの位相差層を含んでもよい。 Examples of the layer having an optical function include a layer having an optically anisotropic substance (for example, an optically anisotropic film). As the layer having optical anisotropy, for example, a polarizer, a retardation layer, viewing angle film, viewing angle limitations (peep prevention) film, a brightness enhancement film, although the optical compensation film and the like, limited to It is not something that is done. The laminate of two or more layers may have two or more selected from these layers having optical anisotropy. In a laminate of two or more layers, all of the layers having optical anisotropy may have different functions, or at least two layers may have the same function. For example, the laminate may include a polarizer and a retardation layer, or may include two retardation layers having different compositions.

光学フィルムは、少なくとも1つの光学的機能を有する層とこの層を保持する基材層(または保護する保護層)とを含んでいてもよい。例えば、偏光板は、少なくともフィルム状の偏光子を備えており、偏光子と偏光子を保護する保護フィルムとで構成されるものであってもよい。 The optical film may include at least one layer having an optical function and a base material layer (or a protective layer that protects the layer). For example, the polarizing plate includes at least a film-shaped polarizing element, and may be composed of a polarizing element and a protective film that protects the polarizing element.

フレキシブル画像表示装置および光学積層体は、それぞれ、光学フィルムとして、少なくとも偏光子または偏光板を備えるものを含むことが好ましい。 It is preferable that the flexible image display device and the optical laminate each include, as an optical film, a film provided with at least a polarizer or a polarizing plate.

偏光子としては、特に制限されず、画像表示装置の分野などで利用されるものが利用できる。偏光子としては、例えば、親水性高分子フィルムに二色性物質を吸着させて一軸延伸したフィルム、ポリエン系配向フィルムが挙げられる。親水性高分子フィルムを構成する親水性高分子としては、例えば、ポリビニルアルコール系樹脂(部分ホルマール化ポリビニルアルコール系樹脂も含む)、エチレン−酢酸ビニル共重合体の部分ケン化物が挙げられる。二色性物質としては、例えば、ヨウ素、二色性染料が挙げられる。ポリエン系配向フィルムを構成する材料としては、例えば、ポリビニルアルコール系樹脂の脱水処理物、ポリ塩化ビニル系樹脂の脱塩酸処理物が挙げられる。 The polarizer is not particularly limited, and those used in the field of image display devices and the like can be used. Examples of the polarizer include a film in which a dichroic substance is adsorbed on a hydrophilic polymer film and uniaxially stretched, and a polyene-based oriented film. Examples of the hydrophilic polymer constituting the hydrophilic polymer film include polyvinyl alcohol-based resins (including partially formalized polyvinyl alcohol-based resins) and partially saponified ethylene-vinyl acetate copolymers. Examples of the dichroic substance include iodine and a dichroic dye. Examples of the material constituting the polyene-based alignment film include a dehydrated product of a polyvinyl alcohol-based resin and a dehydrochlorinated product of a polyvinyl chloride-based resin.

偏光子として、厚みが10μm以下の薄型偏光子を用いてもよい。薄型偏光子としては、例えば、特開昭51−069644号公報、特開2000−338329号公報、国際公開第2010/100917号パンフレット、特許第4691205号公報、特許第4751481号公報に記載されている偏光子が挙げられる。薄型偏光子は、例えば、ポリビニルアルコール系樹脂層と樹脂基材層とを積層させた状態で延伸する工程と、二色性材料により染色する工程とを含む製法により得られる。 As the polarizer, a thin polarizer having a thickness of 10 μm or less may be used. Examples of the thin polarizing element are described in JP-A-51-069644, JP-A-2000-338329, International Publication No. 2010/100917 Pamphlet, Patent No. 46910205, and Patent No. 4751481. Polarizers can be mentioned. The thin polarizer can be obtained, for example, by a production method including a step of stretching a polyvinyl alcohol-based resin layer and a resin base material layer in a laminated state, and a step of dyeing with a dichroic material.

保護フィルムとしては、例えば、透明性、機械的強度、熱安定性、水分遮断性、及び光学等方性に優れる高分子フィルムが用いられる。このような性質を有する高分子材料として、保護フィルムは、例えば、セルロース系樹脂、ポリオレフィン系樹脂(環状ポリオレフィン系樹脂も含む)、アクリル系樹脂、イミド系樹脂(フェニルマレイミド系樹脂も含む)、ポリアミド系樹脂、ポリカーボネート系樹脂、ポリエステル系樹脂(ポリアリーレート系樹脂も含む)、アセテート系樹脂、ポリエーテルスルホン系樹脂、ポリ塩化ビニル系樹脂、ポリ塩化ビニリデン系樹脂、ポリスチレン系樹脂、ポリビニルアルコール系樹脂、スルフィド系樹脂(例えば、ポリフェニレンスルフィド系樹脂)、ポリエーテルエーテルケトン系樹脂、エポキシ系樹脂、およびウレタン系樹脂からなる群より選択される少なくとも一種を含む。しかし、保護フィルムを構成する樹脂は、これらの高分子材料に限定されるものではない。 As the protective film, for example, a polymer film having excellent transparency, mechanical strength, thermal stability, moisture blocking property, and optical isotropic property is used. As the polymer material having such properties, the protective film includes, for example, cellulose-based resin, polyolefin-based resin (including cyclic polyolefin-based resin), acrylic-based resin, imide-based resin (including phenylmaleimide-based resin), and polyamide. Based resin, polycarbonate resin, polyester resin (including polyarylate resin), acetate resin, polyether sulfone resin, polyvinyl chloride resin, polyvinylidene chloride resin, polystyrene resin, polyvinyl alcohol resin , At least one selected from the group consisting of sulfide-based resins (for example, polyphenylene sulfide-based resins), polyether ether ketone-based resins, epoxy-based resins, and urethane-based resins. However, the resin constituting the protective film is not limited to these polymer materials.

光学フィルムは、1層の保護フィルムを含んでいてもよく、2層以上の保護フィルムを含んでもよい。保護フィルムは、光学的機能を有する層(例えば、偏光子)の一方の表面に配置されていてもよく、双方の表面に配置されていてもよい。また、光学フィルムは、一方の表面に保護フィルムが配置された光学的機能を有する層を2層以上含んでもよい。光学フィルムに2層以上の保護フィルムが含まれる場合(例えば、偏光子の双方の表面に保護フィルムが配置される場合)、全ての保護フィルムの組成は、異なっていてもよく、少なくとも2層の保護フィルムにおいて組成が同じであってもよい。 The optical film may include one layer of protective film and may contain two or more layers of protective film. The protective film may be arranged on one surface of a layer having an optical function (for example, a polarizer), or may be arranged on both surfaces. Further, the optical film may include two or more layers having an optical function in which a protective film is arranged on one surface. If the optical film contains more than one layer of protective film (eg, if the protective film is placed on both surfaces of the polarizer), the composition of all protective films may be different, with at least two layers. The composition of the protective film may be the same.

光学フィルムは、偏光子または偏光板に加え、さらに偏光子または偏光板以外の光学的機能を付与する他のフィルム(以下、層Bと称する)を備えていてもよい。層Bとしては、例えば、画像表示装置の分野などで利用されるものが挙げられる。層Bは、例えば、光学異方性フィルムであってもよい。層Bとしては、上記の光学異方性を有する層のうち、偏光子または偏光板以外のものが挙げられる。具体的には、層Bとしては、例えば、位相差層、視野角拡大フィルム、視野角制限(覗き見止)フィルム、輝度向上フィルム、光学補償フィルムが挙げられる。光学フィルムは、このような層Bを1つ含んでいてもよく、2つ以上含んでいてもよい。しかし、層Bは、これらに限定されるものではない。 In addition to the polarizer or the polarizing plate, the optical film may further include another film (hereinafter, referred to as layer B) that imparts an optical function other than the polarizer or the polarizing plate. Examples of the layer B include those used in the field of image display devices. The layer B may be, for example, an optically anisotropic film. Examples of the layer B include layers other than the polarizer or the polarizing plate among the above-mentioned layers having optical anisotropy. Specifically, as the layer B, for example, a phase difference layer, the viewing angle film, viewing angle limitations (peep prevention) film, a brightness enhancement film, an optical compensation film. The optical film may contain one such layer B, or may contain two or more such layers B. However, layer B is not limited to these.

層Bは、保護フィルムを介して偏光板に積層されていてもよく、保護フィルムを介さずに偏光子に積層されていてもよい。偏光板が保護フィルムを有さない場合には、層Bが保護フィルムとしての機能を兼ね備えることになる。 The layer B may be laminated on the polarizing plate via the protective film, or may be laminated on the polarizer without the protective film. When the polarizing plate does not have a protective film, the layer B also functions as a protective film.

光学フィルムの厚みは、例えば、5μm以上500μm以下であり、10μm以上100μm以下であってもよい。 The thickness of the optical film is, for example, 5 μm or more and 500 μm or less, and may be 10 μm or more and 100 μm or less.

偏光板の厚みは、例えば、200μm以下である。より高い屈曲性を確保し易い観点からは、偏光板の厚みは、100μm以下が好ましく、80μm以下または70μm以下がより好ましい。偏光板の厚みは、例えば、10μm以上である。 The thickness of the polarizing plate is, for example, 200 μm or less. From the viewpoint of easily ensuring higher flexibility, the thickness of the polarizing plate is preferably 100 μm or less, more preferably 80 μm or less or 70 μm or less. The thickness of the polarizing plate is, for example, 10 μm or more.

層Bの厚みは、例えば、0.1μm以上100μm以下である。偏光板が保護フィルムを有さない場合(つまり、層Bが保護フィルムとしての機能を兼ね備える場合)には、層Bと偏光板との積層体の厚みが、偏光板の厚みについて記載した範囲になるように層Bの厚みを調節することが好ましい。 The thickness of the layer B is, for example, 0.1 μm or more and 100 μm or less. When the polarizing plate does not have a protective film (that is, when the layer B also functions as a protective film), the thickness of the laminate of the layer B and the polarizing plate is within the range described for the thickness of the polarizing plate. It is preferable to adjust the thickness of the layer B so as to be.

なお、光学フィルムを構成する層は、コーティングなどを利用して隣接する層に直接積層されていてもよい。また、光学フィルムを構成する層は、接着部材または粘着部材を介して隣接する層に積層されていてもよい。例えば、層Bは、偏光板に、接着部材を介して積層されていてもよく、粘着部材を介して積層されていてもよい。また、2つ以上の隣接する層Bを備える場合には、隣接する層B間は、接着部材または粘着部材のいずれを介して積層されていてもよい。 The layers constituting the optical film may be directly laminated on the adjacent layers by using a coating or the like. Further, the layers constituting the optical film may be laminated on adjacent layers via an adhesive member or an adhesive member. For example, the layer B may be laminated on the polarizing plate via an adhesive member, or may be laminated via an adhesive member. When two or more adjacent layers B are provided, the adjacent layers B may be laminated via either an adhesive member or an adhesive member.

(タッチセンサ)
タッチセンサとしては、例えば、画像表示装置の分野などで用いられるものが使用される。タッチセンサとして、例えば、抵抗膜方式、静電容量方式、光学方式、または超音波方式のものが挙げられるが、これらに限定されるものではない。フレキシブル画像表示装置および光学積層体において、タッチセンサとウインドウ部材との間に光学フィルムが存在する場合には、静電容量方式のタッチセンサを用いると高感度が得られ易い。
(Touch sensor)
As the touch sensor, for example, a touch sensor used in the field of an image display device or the like is used. Examples of the touch sensor include, but are not limited to, a resistive film type, a capacitance type, an optical type, and an ultrasonic type. In the flexible image display device and the optical laminate, when an optical film is present between the touch sensor and the window member, it is easy to obtain high sensitivity by using the capacitive touch sensor.

静電容量方式のタッチセンサは、通常、透明導電層を備えている。このようなタッチセンサとしては、例えば、透明導電層と透明基材との積層体が挙げられる。透明基材としては、例えば、透明フィルムが挙げられる。 Capacitive touch sensors usually include a transparent conductive layer. Examples of such a touch sensor include a laminate of a transparent conductive layer and a transparent base material. Examples of the transparent base material include a transparent film.

透明導電層には、特に制限されるものではないが、導電性の金属酸化物、金属ナノワイヤなどが用いられる。金属酸化物としては、例えば、酸化スズを含む酸化インジウム(ITO:Indium Tin Oxide)、アンチモンを含む酸化スズが挙げられる。透明導電層は、金属酸化物または金属で構成される導電性パターンであってもよい。導電性パターンの形状としては、ストライプ状、スクエア状、格子状などが挙げられるが、これらに限定されるものではない。 The transparent conductive layer is not particularly limited, but a conductive metal oxide, metal nanowires, or the like is used. Examples of the metal oxide include indium oxide (ITO: Indium Tin Oxide) containing tin oxide and tin oxide containing antimony. The transparent conductive layer may be a conductive pattern composed of a metal oxide or a metal. Examples of the shape of the conductive pattern include, but are not limited to, a striped shape, a square shape, and a grid shape.

透明導電層の表面抵抗値は、例えば、0.1Ω/□以上1000Ω/□以下であり、0.5Ω/□以上500Ω/□以下であってもよい。 The surface resistance value of the transparent conductive layer may be, for example, 0.1 Ω / □ or more and 1000 Ω / □ or less, and may be 0.5 Ω / □ or more and 500 Ω / □ or less.

透明導電層の厚みは、例えば、0.005μm以上10μm以下であり、0.01μm以上3μm以下であってもよい。 The thickness of the transparent conductive layer is, for example, 0.005 μm or more and 10 μm or less, and may be 0.01 μm or more and 3 μm or less.

透明フィルムとしては、例えば、透明樹脂フィルムが用いられる。透明樹脂フィルムを構成する樹脂としては、ポリエステル系樹脂(ポリアリーレート系樹脂も含む)、アセテート系樹脂、ポリエーテルスルホン系樹脂、ポリカーボネート系樹脂、ポリアミド系樹脂、ポリイミド系樹脂、ポリオレフィン系樹脂、アクリル系樹脂、ポリ塩化ビニル系樹脂、ポリ塩化ビニリデン系樹脂、ポリスチレン系樹脂、ポリビニルアルコール系樹脂、スルフィド系樹脂(例えば、ポリフェニレンスルフィド系樹脂)、ポリエーテルエーテルケトン系樹脂、セルロース系樹脂、エポキシ系樹脂、ウレタン系樹脂等が挙げられる。透明樹脂フィルムは、これらの樹脂を一種含んでもよく、二種以上含んでもよい。これらの樹脂のうち、ポリエステル系樹脂、ポリイミド系樹脂及びポリエーテルスルホン系樹脂が好ましい。しかし、透明樹脂フィルムを構成する樹脂は、これらの樹脂に限定されるものではない。 As the transparent film, for example, a transparent resin film is used. The resins constituting the transparent resin film include polyester resins (including polyarylate resins), acetate resins, polyether sulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, and acrylics. Based resin, polyvinyl chloride resin, vinylidene chloride resin, polystyrene resin, polyvinyl alcohol resin, sulfide resin (for example, polyphenylene sulfide resin), polyether ether ketone resin, cellulose resin, epoxy resin , Urethane-based resin and the like. The transparent resin film may contain one kind of these resins, or may contain two or more kinds of these resins. Of these resins, polyester-based resins, polyimide-based resins and polyether sulfone-based resins are preferable. However, the resin constituting the transparent resin film is not limited to these resins.

透明導電層と透明基材との密着性を高める観点から、透明基材としては、表面処理されたものを用いてもよい。表面処理としては、公知のものが採用できる。また、必要に応じて、透明導電層の積層に先立って、透明基材には、例えば、除塵または清浄化処理(溶剤または超音波などを利用した洗浄処理など)を行ってもよい。 From the viewpoint of enhancing the adhesion between the transparent conductive layer and the transparent base material, a surface-treated transparent base material may be used. As the surface treatment, a known one can be adopted. Further, if necessary, the transparent base material may be subjected to, for example, a dust removal or cleaning treatment (cleaning treatment using a solvent, ultrasonic waves, or the like) prior to laminating the transparent conductive layer.

タッチセンサには、必要に応じて、透明導電層および透明基材以外の他の層(以下、層Cと称する)を設けてもよい。例えば、透明導電層と透明基材との間に、層Cとして、アンダーコート層またはオリゴマー析出防止層を設けてもよい。また、透明導電層および透明基材の少なくとも一方の表面に、層Cを積層してもよい。層Cとしては、所望の機能を有する機能層(例えば、上記の光学的機能を付与するフィルム(光学異方性フィルムなど)、上記の光学的機能を有する層)、加飾付き基材フィルムなどが挙げられる。加飾付き基材フィルムは、例えば、透明導電層の表面に積層される。ただし、層Cはこれらの層に限定されるものではない。層Cは、必要に応じて、接着部材または粘着部材を介して、透明導電層または透明基材に積層してもよい。 If necessary, the touch sensor may be provided with a layer other than the transparent conductive layer and the transparent base material (hereinafter, referred to as layer C). For example, an undercoat layer or an oligomer precipitation prevention layer may be provided as the layer C between the transparent conductive layer and the transparent base material. Further, the layer C may be laminated on at least one surface of the transparent conductive layer and the transparent base material. The layer C includes a functional layer having a desired function (for example, a film imparting the above optical function (optically anisotropic film or the like), a layer having the above optical function), a decorative base film, or the like. Can be mentioned. The decorative base film is laminated on the surface of the transparent conductive layer, for example. However, layer C is not limited to these layers. The layer C may be laminated on the transparent conductive layer or the transparent base material via the adhesive member or the adhesive member, if necessary.

タッチセンサ全体の厚みは、例えば、5μm以上250μm以下であり、10μm以上200μm以下であってもよい。 The thickness of the entire touch sensor is, for example, 5 μm or more and 250 μm or less, and may be 10 μm or more and 200 μm or less.

(第3部材)
フレキシブル画像表示装置および光学積層体において、第3部材は、ウインドウ部材に、第1部材および第2部材を介して積層されている。そして、第2部材と第3部材との間には、粘着部材が介在した状態である。フレキシブル画像表示装置の第3部材を、第3A部材と称する。第3A部材は、少なくともパネル部材を含む。光学積層体の第3部材を、第3B部材と称する。第3B部材は、少なくともセパレータ(第2セパレータ)を含む。光学積層体は、セパレータを剥離した状態でフレキシブル画像表示装置に含まれる。第3B部材には、パネル部材およびタッチセンサ付パネル部材のいずれも含まれない。第3A部材および第3B部材のそれぞれは積層体であってもよい。第3A部材および第3B部材のそれぞれには、接着部材または粘着部材が含まれていてもよい。
(Third member)
In the flexible image display device and the optical laminate, the third member is laminated on the window member via the first member and the second member. An adhesive member is interposed between the second member and the third member. The third member of the flexible image display device is referred to as a third A member. The third A member includes at least a panel member. The third member of the optical laminate is referred to as a third B member. The third B member includes at least a separator (second separator). The optical laminate is included in the flexible image display device with the separator peeled off. The third B member does not include either a panel member or a panel member with a touch sensor. Each of the third A member and the third B member may be a laminated body. Each of the third A member and the third B member may include an adhesive member or an adhesive member.

第3A部材は、少なくともパネル部材を含んでいればよい。第3A部材は、例えば、パネル部材とパネル部材を保護する保護部材との積層体であってもよい。第3A部材が、保護部材を含む場合、保護部材は、通常、パネル部材の第2部材側とは反対側に積層されている。つまり、パネル部材の視認側とは反対側に保護部材が設けられている。しかし、これらは単なる例示であり、第3A部材はこれらに限定されるものではない。第3A部材が積層体である場合、積層体を構成する隣接する層(または部材、例えば、パネル部材と保護部材と)は、接着部材または粘着部材を介して積層されていてもよい。 The third A member may include at least a panel member. The third A member may be, for example, a laminated body of a panel member and a protective member that protects the panel member. When the third A member includes a protective member, the protective member is usually laminated on the side opposite to the second member side of the panel member. That is, the protective member is provided on the side opposite to the visible side of the panel member. However, these are merely examples, and the third A member is not limited thereto. When the third A member is a laminated body, adjacent layers (or members, for example, a panel member and a protective member) constituting the laminated body may be laminated via an adhesive member or an adhesive member.

第3A部材の弾性率(GPa)を、E3とし、第3A部材の厚み(mm)を、T3とする。第3A部材は、下式を充足することが好ましい。
0.01(kN/mm)≦E3×T3≦0.35(kN/mm)
第3A部材において、弾性率と厚みとの積がこのような範囲であることで、粘着部材の厚みを上述のように制御することによる効果がさらに得られ易くなる。
The elastic modulus (GPa) of the third A member is E3, and the thickness (mm) of the third A member is T3. The third A member preferably satisfies the following equation.
0.01 (kN / mm) ≤ E3 x T3 ≤ 0.35 (kN / mm)
In the third A member, when the product of the elastic modulus and the thickness is in such a range, the effect of controlling the thickness of the adhesive member as described above can be further easily obtained.

光学積層体における第3B部材は、少なくともセパレータを含んでいればよい。第3B部材をセパレータのみで構成してもよい。第3B部材は、第2部材の第1部材側とは反対側に配置された粘着部材にセパレータが接触するように第2部材と積層される。そして、光学積層体からセパレータを剥離して、露出した粘着部材を、第3A部材(具体的には、パネル部材またはパネル部材を含む積層体)に貼り付けることによりフレキシブル画像表示装置が形成される。 The third B member in the optical laminate may include at least a separator. The third B member may be composed of only a separator. The third B member is laminated with the second member so that the separator comes into contact with the adhesive member arranged on the side opposite to the first member side of the second member. Then, the separator is peeled off from the optical laminate, and the exposed adhesive member is attached to the third A member (specifically, the panel member or the laminate including the panel member) to form a flexible image display device. ..

(パネル部材)
パネル部材は、例えば、少なくとも画像表示パネルを含む。画像表示パネルの視認側には、封止部材(薄膜封止層など)が配置されていてもよい。封止部材は、通常、画像表示パネルの視認側の表面に直接配置されている。
(Panel member)
The panel member includes, for example, at least an image display panel. A sealing member (thin film sealing layer or the like) may be arranged on the visual side of the image display panel. The sealing member is usually arranged directly on the visible surface of the image display panel.

画像表示パネルとしては、公知のものが使用される。画像表示パネルとしては、例えば、有機エレクトロルミネッセンス(EL:Electro Luminescence)パネルが挙げられる。 As the image display panel, a known one is used. Examples of the image display panel include an organic electroluminescence (EL) panel.

(保護部材)
保護部材としては、例えば、パネル部材を保持または保護するシートまたはフィルム(もしくは基板)が挙げられる。保護部材は、パネル部材を保持するとともに、パネル部材を保護するための適度な強度、およびフレキシブル画像表示装置の屈曲性を妨げない適度な柔軟性を有するものであればよい。保護部材としては、樹脂シートなどが用いられる。樹脂シートの材質は、特に制限されず、例えば、画像表示パネルの種類に応じて適宜選択できる。
(Protective member)
Examples of the protective member include a sheet or film (or substrate) that holds or protects the panel member. The protective member may be one that holds the panel member, has an appropriate strength for protecting the panel member, and has an appropriate flexibility that does not hinder the flexibility of the flexible image display device. As the protective member, a resin sheet or the like is used. The material of the resin sheet is not particularly limited, and can be appropriately selected depending on the type of the image display panel, for example.

(タッチセンサ付パネル部材)
タッチセンサ付パネル部材(具体的には、第1タッチセンサ付パネル部材および第3A部材に含まれる第2タッチセンサ付パネル部材のそれぞれ)は、タッチセンサとパネル部材とが一体化したものである。このようなタッチセンサ付パネル部材には、例えば、有機発光ダイオード(OLED:Organic Light Emitting Diode)の薄膜封止層上にメタルメッシュ電極の制電容量式タッチセンサを形成した構成のものも包含される。タッチセンサとしては、上記の説明を参照してもよい。
(Panel member with touch sensor)
The panel member with a touch sensor (specifically, each of the panel member with a first touch sensor and the panel member with a second touch sensor included in the third A member) is an integral body of the touch sensor and the panel member. .. Such a panel member with a touch sensor includes, for example, a structure in which an antistatic capacity type touch sensor of a metal mesh electrode is formed on a thin film sealing layer of an organic light emitting diode (OLED). LED. As the touch sensor, the above description may be referred to.

パネル部材は、例えば、少なくとも画像表示パネルを含む。画像表示パネルの視認側には、封止部材(薄膜封止層など)が配置されていてもよい。封止部材は、通常、画像表示パネルの視認側の表面に直接配置されている。 The panel member includes, for example, at least an image display panel. A sealing member (thin film sealing layer or the like) may be arranged on the visual side of the image display panel. The sealing member is usually arranged directly on the visible surface of the image display panel.

画像表示パネルとしては、公知のものが使用される。画像表示パネルとしては、例えば、有機エレクトロルミネッセンス(EL:Electro Luminescence)パネルが挙げられる。 As the image display panel, a known one is used. Examples of the image display panel include an organic electroluminescence (EL) panel.

タッチセンサ付パネル部材は、保護部材を備えていてもよい。保護部材としては、例えば、パネル部材を保持または保護するシートまたはフィルム(もしくは基板)が挙げられる。保護部材は、パネル部材を保持するとともに、パネル部材を保護するための適度な強度、およびフレキシブル画像表示装置の屈曲性を妨げない適度な柔軟性を有するものであればよい。保護部材としては、樹脂シートなどが用いられる。樹脂シートの材質は、特に制限されず、例えば、画像表示パネルの種類に応じて適宜選択できる。 The panel member with a touch sensor may include a protective member. Examples of the protective member include a sheet or film (or substrate) that holds or protects the panel member. The protective member may be one that holds the panel member, has an appropriate strength for protecting the panel member, and has an appropriate flexibility that does not hinder the flexibility of the flexible image display device. As the protective member, a resin sheet or the like is used. The material of the resin sheet is not particularly limited, and can be appropriately selected depending on the type of the image display panel, for example.

タッチセンサ付パネル部材の弾性率(GPa)を、Epとし、タッチセンサ付パネル部材の厚み(mm)を、Tpとする。このとき、タッチセンサ付パネル部材は、下式を充足することが好ましい。
0.01≦Ep×Tp≦0.35
タッチセンサ付パネル部材において、弾性率と厚みとの積がこのような範囲であることで、各粘着部材の厚みを上述のように制御することによる効果がさらに得られ易くなる。なお、Ep×Tpの単位は、kN/mmである。
The elastic modulus (GPa) of the panel member with a touch sensor is Ep, and the thickness (mm) of the panel member with a touch sensor is Tp. At this time, the panel member with the touch sensor preferably satisfies the following formula.
0.01 ≤ Ep x Tp ≤ 0.35
In the panel member with a touch sensor, when the product of the elastic modulus and the thickness is in such a range, the effect of controlling the thickness of each adhesive member as described above can be further easily obtained. The unit of Ep × Tp is kN / mm.

(セパレータ)
セパレータ(具体的には、第1セパレータおよび第3B部材に含まれる第2セパレータのそれぞれ)としては、例えば、基材シートと基材シートの少なくとも一方の表面に配された剥離剤とを備える剥離シートが用いられる。セパレータは、剥離剤が粘着部材と接触した状態で配置される。より具体的には、第1セパレータは、第1部材のウインドウ部材とは反対側に配置された粘着部材と接触した状態で配置される。第2セパレータは、第2部材の第1部材側とは反対側に配置された粘着部材と接触した状態で配置される。
(Separator)
The separator (specifically, each of the first separator and the second separator included in the third B member) includes, for example, a base sheet and a release agent arranged on at least one surface of the base sheet. Sheets are used. The separator is arranged with the release agent in contact with the adhesive member. More specifically, the first separator is arranged in contact with the adhesive member arranged on the side opposite to the window member of the first member. The second separator is arranged in contact with the adhesive member arranged on the side opposite to the first member side of the second member.

基材シートとしては、光学積層体の第1セパレータまたは第3B部材を除く構成を保持するとともに、適度な強度および柔軟性を有し、剥離剤の層が容易に形成できるものであればよい。基材シートとしては、樹脂フィルム、紙、またはこれらの積層体などが用いられる。基材シートの材質は、剥離剤の種類、光学積層体の構成などに応じて決定される。樹脂フィルムとしては、例えば、ポリエステルフィルム(ポリエチレンテレフタレートフィルムなど)、ポリオレフィンフィルム(ポリプロピレンフィルムなど)を用いてもよい。基材シートの厚みも特に制限されず、所望の剥離性を考慮して選択できる。剥離剤としては、公知のものが使用でき、粘着部材のセパレータへの残存量が少ないものを選択することが好ましい。例えば、シリコーン系剥離剤、フッ素系剥離剤を用いてもよい。 The base sheet may have a structure other than the first separator or the third B member of the optical laminate, have appropriate strength and flexibility, and can easily form a release agent layer. As the base sheet, a resin film, paper, a laminate thereof, or the like is used. The material of the base sheet is determined according to the type of release agent, the composition of the optical laminate, and the like. As the resin film, for example, a polyester film (polyethylene terephthalate film or the like) or a polyolefin film (polypropylene film or the like) may be used. The thickness of the base sheet is not particularly limited, and can be selected in consideration of desired peelability. As the release agent, a known one can be used, and it is preferable to select one having a small residual amount of the adhesive member on the separator. For example, a silicone-based release agent or a fluorine-based release agent may be used.

(加飾層)
加飾層は、例えば、ウインドウ部材とタッチセンサまたはタッチセンサ付パネル部材(より具体的には、第1タッチセンサ付パネル部材または第2タッチセンサ付パネル部材)との間において、少なくとも1層の粘着部材と接触するように配置される。また、第1部材内に粘着部材が含まれる場合には、この粘着部材と接触するように配置されていてもよい。例えば、ウインドウ部材の第1部材側の表面、および第1部材のウインドウ部材側の表面の少なくとも一方に加飾層を形成してもよい。また、第1部材が光学フィルムである場合、第1部材の第1積層体側または第1タッチセンサ付パネル部材側(あるいは第1セパレータ側)の表面、および第2部材が光学フィルムの場合には第2部材の第3A部材側(または第3B部材側)の表面の少なくとも一方に加飾層を形成してもよい。第1部材が光学フィルムであり、第1部材内に粘着部材の層が含まれる場合には、この粘着部材の層を挟持する層のうち、少なくとも一方の層の粘着部材と接触する表面に加飾層を形成してもよい。第2部材が光学フィルムであり、第2部材内に粘着部材の層が含まれる場合には、この粘着部材の層を挟持する層のうち、少なくとも一方の層の粘着部材と接触する表面に加飾層を形成してもよい。加飾層は、これらの部材および層の表面のうち少なくとも1つの表面に形成されていればよく、2つ以上の表面に形成されていてもよい。加飾層は、画像が表示される表示部の外周に駆動素子またはタッチセンサの引出配線が外部から視認されないように、通常、フレーム状のパターンで設けられる。しかし、加飾層の形状はフレーム状に限定されるものではなく、引出配線などを隠蔽できる形状であればよい。
(Decorative layer)
The decorative layer is, for example, at least one layer between the window member and the touch sensor or the panel member with the touch sensor (more specifically, the panel member with the first touch sensor or the panel member with the second touch sensor). Arranged so as to come into contact with the adhesive member. Further, when the adhesive member is included in the first member, it may be arranged so as to come into contact with the adhesive member. For example, a decorative layer may be formed on at least one of the surface of the window member on the first member side and the surface of the first member on the window member side. When the first member is an optical film, the surface of the first member on the first laminated body side or the panel member side with the first touch sensor (or the first separator side), and when the second member is an optical film, A decorative layer may be formed on at least one of the surfaces of the second member on the third A member side (or the third B member side). When the first member is an optical film and the first member includes a layer of the adhesive member, it is added to the surface of at least one of the layers sandwiching the layer of the adhesive member in contact with the adhesive member. A decorative layer may be formed. When the second member is an optical film and the second member includes a layer of the adhesive member, it is added to the surface of at least one of the layers sandwiching the layer of the adhesive member in contact with the adhesive member. A decorative layer may be formed. The decorative layer may be formed on at least one surface of the surfaces of these members and layers, and may be formed on two or more surfaces. The decorative layer is usually provided in a frame-like pattern on the outer periphery of the display unit on which the image is displayed so that the lead wiring of the drive element or the touch sensor is not visible from the outside. However, the shape of the decorative layer is not limited to the frame shape, and may be any shape that can hide the lead-out wiring and the like.

加飾層には、視認側からの光を反射しないことに加え、視認側とは反対側からの光を遮蔽することが求められる。このような加飾層としては、例えば、インキ層、金属薄膜、金属微粒子を含む薄膜で構成される。金属微粒子を含む薄膜は、例えば、金属微粒子とバインダ樹脂とを含む。加飾層は、単層構造であってもよく、積層構造であってもよい。積層構造の加飾層は、例えば、インキ層、金属薄膜および金属微粒子を含む薄膜から選択される少なくとも2つの積層体であってもよい。この積層体には、組成の異なる2つ以上のインキ層、組成の異なる2つ以上の金属薄膜、または組成の異なる2つ以上の金属微粒子を含む薄膜の積層体も含まれる。 In addition to not reflecting the light from the viewing side, the decorative layer is required to shield the light from the side opposite to the viewing side. Such a decorative layer is composed of, for example, an ink layer, a metal thin film, and a thin film containing metal fine particles. The thin film containing the metal fine particles includes, for example, the metal fine particles and the binder resin. The decorative layer may have a single-layer structure or a laminated structure. The decorative layer of the laminated structure may be, for example, at least two laminated bodies selected from an ink layer, a metal thin film, and a thin film containing metal fine particles. The laminate also includes a laminate of two or more ink layers having different compositions, two or more metal thin films having different compositions, or a thin film containing two or more metal fine particles having different compositions.

加飾層の厚みは、例えば、20μm以下であり、15μm以下であってもよい。加飾層による段差を粘着部材により解消し易い観点からは、加飾層の厚みは、10μm以下が好ましく、8μm以下または5μm以下であってもよい。また、加飾層の厚みがこのような範囲である場合、フレキシブル画像表示装置および光学積層体の高い耐屈曲性を確保し易い。引出配線のより高い隠蔽効果を確保する観点からは、加飾層の厚みは、10nm以上であることが好ましく、30nm以上または50nm以上がより好ましい。これらの下限値と上限値とは任意に組み合わせることができる。 The thickness of the decorative layer is, for example, 20 μm or less, and may be 15 μm or less. From the viewpoint that the step due to the decorative layer can be easily eliminated by the adhesive member, the thickness of the decorative layer is preferably 10 μm or less, and may be 8 μm or less or 5 μm or less. Further, when the thickness of the decorative layer is in such a range, it is easy to secure high bending resistance of the flexible image display device and the optical laminate. From the viewpoint of ensuring a higher concealing effect of the lead wiring, the thickness of the decorative layer is preferably 10 nm or more, more preferably 30 nm or more or 50 nm or more. These lower limit values and upper limit values can be arbitrarily combined.

加飾層は、例えば、上記の加飾層が形成される部材または層の表面に、加飾層の構成成分を含むコーティング剤を塗布することにより形成してもよい。また、加飾層は、上記の加飾層が形成される部材または層の表面に、気相法で構成成分を堆積させることにより形成してもよい。金属薄膜の場合、特に、気相法を利用することで厚みの小さな加飾層を容易に形成することができる。気相法としては、スパッタ法、真空蒸着法、化学気相成長(CVD:Chemical Vapor Deposition)法、電子線蒸着法などが挙げられる。 The decorative layer may be formed, for example, by applying a coating agent containing a component of the decorative layer to the surface of the member or layer on which the decorative layer is formed. Further, the decorative layer may be formed by depositing constituent components on the surface of the member or layer on which the decorative layer is formed by a vapor phase method. In the case of a metal thin film, in particular, a decorative layer having a small thickness can be easily formed by using the vapor phase method. Examples of the gas phase method include a sputtering method, a vacuum deposition method, a chemical vapor deposition (CVD) method, and an electron beam deposition method.

上記の加飾層が形成される部材または層の表面には、コーティング剤の塗布に先立ってプライマー層が配置されていてもよい。例えば、加飾層が、ウインドウ部材の第1部材側の表面に設けられている場合、加飾層とウインドウ部材の第1部材側の表面との間には、プライマー層が配置されていてもよい。加飾層が、第1部材の第1積層体側または第1タッチセンサ付パネル部材側(あるいは第1セパレータ側)の表面に設けられている場合、加飾層と第1部材の第1積層体側または第1タッチセンサ付パネル部材側(あるいは第1セパレータ側)の表面との間には、プライマー層が配置されていてもよい。プライマー層は、例えば、金属化合物(金属酸化物、金属窒化物、金属炭化物、金属硫化物など)、および樹脂材料からなる群より選択される少なくとも一種を含む。プライマー層は透明であることが好ましい。 A primer layer may be arranged on the surface of the member or layer on which the decorative layer is formed prior to application of the coating agent. For example, when the decorative layer is provided on the surface of the window member on the first member side, even if the primer layer is arranged between the decorative layer and the surface of the window member on the first member side. Good. When the decorative layer is provided on the surface of the first laminated body side of the first member or the panel member side with the first touch sensor (or the first separator side), the decorative layer and the first laminated body side of the first member Alternatively, a primer layer may be arranged between the surface of the panel member with the first touch sensor (or the side of the first separator). The primer layer contains, for example, at least one selected from the group consisting of metal compounds (metal oxides, metal nitrides, metal carbides, metal sulfides, etc.) and resin materials. The primer layer is preferably transparent.

粘着部材により加飾層の段差を吸収し易いことに加え、プライマー層による光学的な影響を抑制し易い観点から、プライマー層の厚みは小さい方が好ましい。プライマー層の厚みは、例えば、500nm以下であり、100nm以下または30nm以下が好ましい。 The thickness of the primer layer is preferably small from the viewpoint that the adhesive member easily absorbs the step difference of the decorative layer and the optical influence of the primer layer can be easily suppressed. The thickness of the primer layer is, for example, 500 nm or less, preferably 100 nm or less or 30 nm or less.

フレキシブル画像表示装置および光学積層体は、例えば、構成部材を、粘着部材を各部材間(および必要に応じて各部材を構成する層間)に配置しながら積層することにより作製される。積層の順序は特に制限されない。 The flexible image display device and the optical laminate are manufactured, for example, by laminating the constituent members while arranging the adhesive members between the respective members (and, if necessary, between the layers constituting the respective members). The stacking order is not particularly limited.

例えば、ウインドウ部材と第1部材とをこれらの部材間に粘着部材を介在させた状態で積層し、次いで、第1部材と第2部材とをこれらの部材間に粘着部材を介在させた状態で積層してもよい。また、第1部材と第2部材とをこれらの部材間に粘着部材を介在させた状態で積層した後に、第1部材とウインドウ部材とをこれらの部材間に粘着部材を介在させた状態で積層してもよい。各粘着部材は、各粘着部材を挟持する部材の一方に予め貼り付けておくことが好ましい。 For example, the window member and the first member are laminated with the adhesive member interposed therebetween, and then the first member and the second member are laminated with the adhesive member interposed between the members. It may be laminated. Further, after laminating the first member and the second member with the adhesive member interposed between the members, the first member and the window member are laminated with the adhesive member interposed between the members. You may. It is preferable that each adhesive member is previously attached to one of the members that sandwich each adhesive member.

光学積層体では、第2部材を第1部材と積層する前に、第2部材の第1部材側とは反対側の面に粘着部材を配置してもよい。また、第2部材を第1部材と積層した後の適当な段階で、第2部材の第1部材側とは反対側の面に粘着部材を配置してもよい。光学積層体では、第2部材の第1部材側とは反対側の面に配置される粘着部材には、第2部材の面に粘着部材を配置する前または配置した後にセパレータが積層される。 In the optical laminated body, the adhesive member may be arranged on the surface of the second member opposite to the first member side before laminating the second member with the first member. Further, the adhesive member may be arranged on the surface of the second member opposite to the first member side at an appropriate stage after the second member is laminated with the first member. In the optical laminated body, the separator is laminated on the adhesive member arranged on the surface of the second member opposite to the first member side before or after the adhesive member is arranged on the surface of the second member.

フレキシブル画像表示装置は、光学積層体を予め作製し、光学積層体から第3B部材(より具体的には、セパレータ)を剥離し、露出した粘着部材を、第3A部材に貼り付けることにより作製してもよい。また、第3A部材と第2部材とをこれらの間に粘着部材を介在するように積層させた後、第2部材に第1部材をこれらの間に粘着部材が介在するように積層し、次いで、第1部材にウインドウ部材をこれらの間に粘着部材が介在するように積層することによりフレキシブル画像表示装置を作製してもよい。また、第3A部材と第2部材との積層体と、ウインドウ部材と第1部材との積層体とを予め作製し、これらの積層体を、第1部材と第2部材との間に粘着部材を介在させた状態で積層させてもよい。 The flexible image display device is manufactured by preparing an optical laminate in advance, peeling the third B member (more specifically, a separator) from the optical laminate, and attaching the exposed adhesive member to the third A member. You may. Further, the third A member and the second member are laminated so that the adhesive member is interposed between them, and then the first member is laminated on the second member so that the adhesive member is interposed between them, and then. A flexible image display device may be produced by laminating a window member on a first member so that an adhesive member is interposed between them. Further, a laminated body of the third A member and the second member and a laminated body of the window member and the first member are prepared in advance, and these laminated bodies are placed between the first member and the second member. May be laminated in a state of interposing.

これらの製造方法は、単なる例示であり、これらに限定されるものではない。フレキシブル画像表示装置または光学積層体がタッチセンサ付パネル部材を備える場合にも、これらの製造方法に準じて、各部材を積層させることで作製することができる。 These manufacturing methods are merely examples, and are not limited thereto. Even when the flexible image display device or the optical laminate includes a panel member with a touch sensor, it can be manufactured by laminating each member according to these manufacturing methods.

図1は、本発明の上記側面に係る第1実施形態のフレキシブル画像表示装置の概略断面図である。フレキシブル画像表示装置1は、ウインドウ部材11と、第1部材としての光学フィルム12と、第2部材としてのタッチセンサ13と、第3A部材としてのパネル部材14との積層体を備える。第2部材であるタッチセンサ13と第3A部材であるパネル部材14との積層体が第1積層体Lに相当する。光学フィルム12とウインドウ部材11とは、光学フィルム12とウインドウ部材11との間に粘着部材21が介在した状態で積層されている。タッチセンサ13は、光学フィルム12を介してウインドウ部材11に積層されている。光学フィルム12とタッチセンサ13との間には、粘着部材22が介在している。パネル部材14は、光学フィルム12およびタッチセンサ13を介して、ウインドウ部材11に積層されている。タッチセンサ13とパネル部材14との間には、粘着部材23が介在している。図1におけるパネル部材14を除く構成とセパレータ(図示せず)との積層体が、光学積層体に相当する。 FIG. 1 is a schematic cross-sectional view of the flexible image display device of the first embodiment according to the above aspect of the present invention. The flexible image display device 1 includes a laminated body of a window member 11, an optical film 12 as a first member, a touch sensor 13 as a second member, and a panel member 14 as a third A member. The laminated body of the touch sensor 13 which is the second member and the panel member 14 which is the third A member corresponds to the first laminated body L. The optical film 12 and the window member 11 are laminated with the adhesive member 21 interposed between the optical film 12 and the window member 11. The touch sensor 13 is laminated on the window member 11 via the optical film 12. An adhesive member 22 is interposed between the optical film 12 and the touch sensor 13. The panel member 14 is laminated on the window member 11 via the optical film 12 and the touch sensor 13. An adhesive member 23 is interposed between the touch sensor 13 and the panel member 14. The laminated body of the structure excluding the panel member 14 and the separator (not shown) in FIG. 1 corresponds to an optical laminated body.

ウインドウ部材11は、例えば、ウインドウフィルム111と、ウインドウフィルム111に積層されたハードコート層112とを備えている。ハードコート層112は、ウインドウ部材11の第1部材(光学フィルム12)側とは反対側(より具体的には、ウインドウフィルム111の第1部材側とは反対側の表面)に設けられている。そして、ウインドウ部材11の弾性率E0と厚みT0との積は、E0×T0>0.32(kN/mm)を充足する。 The window member 11 includes, for example, a window film 111 and a hard coat layer 112 laminated on the window film 111. The hard coat layer 112 is provided on the side of the window member 11 opposite to the first member (optical film 12) side (more specifically, the surface of the window film 111 opposite to the first member side). .. The product of the elastic modulus E0 of the window member 11 and the thickness T0 satisfies E0 × T0> 0.32 (kN / mm).

光学フィルム12は、偏光子121および保護フィルム122で構成される偏光板と位相差層123とを備える。位相差層123は、第2部材であるタッチセンサ13側に配置されており、偏光板の偏光子121側に積層されている。 The optical film 12 includes a polarizing plate composed of a polarizing element 121 and a protective film 122, and a retardation layer 123. The retardation layer 123 is arranged on the touch sensor 13 side, which is the second member, and is laminated on the polarizer 121 side of the polarizing plate.

タッチセンサ13は、透明導電層131と透明基材としての透明フィルム(タッチセンサフィルム)132とを含む。タッチセンサ13は、透明導電層131が光学フィルム12とタッチセンサ13との間に配置された粘着部材22と接触するように配置されている。 The touch sensor 13 includes a transparent conductive layer 131 and a transparent film (touch sensor film) 132 as a transparent base material. The touch sensor 13 is arranged so that the transparent conductive layer 131 comes into contact with the adhesive member 22 arranged between the optical film 12 and the touch sensor 13.

パネル部材14は、有機ELパネル(有機ELディスプレイ)141と、薄膜封止層142とを備える。パネル部材14は、薄膜封止層142がタッチセンサ13とパネル部材14との間に配置された粘着部材23と接触するように配置されている。 The panel member 14 includes an organic EL panel (organic EL display) 141 and a thin film sealing layer 142. The panel member 14 is arranged so that the thin film sealing layer 142 comes into contact with the adhesive member 23 arranged between the touch sensor 13 and the panel member 14.

フレキシブル画像表示装置1および光学積層体では、E0×T0>0.32(kN/mm)であり、粘着部材21〜23のうち、少なくとも1層の厚みが20μm以上の条件を満たすように制御されている。また、粘着部材21〜23のうち、ウインドウ部材側からn番目の層および(n+1)番目の層の少なくとも一方の厚みが、10μm以上の条件を満たすように、制御されている。そのため、高温環境下でフレキシブル画像表示装置を繰り返し屈曲させても、積層された部材間における高い接着性を確保することができる。また、フレキシブル画像表示装置1および光学積層体のウインドウ部材11側の表面において、比較的高い鉛筆硬度を確保することもできる。 In the flexible image display device 1 and the optical laminate, E0 × T0> 0.32 (kN / mm), and the thickness of at least one of the adhesive members 21 to 23 is controlled so as to satisfy the condition of 20 μm or more. ing. Further, among the adhesive members 21 to 23, the thickness of at least one of the nth layer and the (n + 1) th layer from the window member side is controlled so as to satisfy the condition of 10 μm or more. Therefore, even if the flexible image display device is repeatedly bent in a high temperature environment, high adhesiveness between the laminated members can be ensured. Further, it is possible to secure a relatively high pencil hardness on the surface of the flexible image display device 1 and the optical laminate on the window member 11 side.

図1では、第1部材(光学フィルム12)の第2部材(タッチセンサ13)側の表面にフレーム状の加飾層30が設けられている。この場合、加飾層30が接触する粘着部材(具体的には、粘着部材22)の厚みを10μm以上とすることで、加飾層30による段差を効果的に吸収することができる。 In FIG. 1, a frame-shaped decorative layer 30 is provided on the surface of the first member (optical film 12) on the second member (touch sensor 13) side. In this case, by setting the thickness of the adhesive member (specifically, the adhesive member 22) to which the decorative layer 30 comes into contact to be 10 μm or more, the step caused by the decorative layer 30 can be effectively absorbed.

なお、図1では、加飾層30が、光学フィルム12のタッチセンサ13側の表面に形成される場合を示したが、この場合に限定されない。加飾層30は、ウインドウ部材11の第1部材(光学フィルム12)側の表面に設けられていてもよい。 Note that FIG. 1 shows a case where the decorative layer 30 is formed on the surface of the optical film 12 on the touch sensor 13 side, but the case is not limited to this case. The decorative layer 30 may be provided on the surface of the window member 11 on the first member (optical film 12) side.

図1では、第1部材が光学フィルム12であり、第2部材がタッチセンサ13であり、第3A部材がパネル部材である場合を示した。しかし、この場合に限らず、第1部材としてタッチセンサを、ウインドウ部材11に積層させ、第2部材として光学フィルムを、タッチセンサを介してウインドウ部材11に積層させてもよい。また、第3A部材として、上述のようなパネル部材を含む積層体を用いてもよい。 FIG. 1 shows a case where the first member is an optical film 12, the second member is a touch sensor 13, and the third A member is a panel member. However, not limited to this case, the touch sensor may be laminated on the window member 11 as the first member, and the optical film as the second member may be laminated on the window member 11 via the touch sensor. Further, as the third A member, a laminated body including the panel member as described above may be used.

図2は、第2実施形態のフレキシブル画像表示装置の概略断面図である。フレキシブル画像表示装置101は、ウインドウ部材11と、第1部材としての光学フィルム12Aと、第1積層体Lとの積層体を備える。第1積層体Lは、第2部材である光学フィルム12Bと第3A部材である第2タッチセンサ付パネル部材15Bとが積層された構造を有する。ウインドウ部材11と光学フィルム12Aとの間には粘着部材21が介在している。光学フィルム12Aと第1積層体Lとの間には粘着部材22が介在し、光学フィルム12Bと第2タッチセンサ付パネル部材15Bとの間には粘着部材23が介在している。第1部材である光学フィルム12Aおよび第1積層体Lの構成以外は、第1実施形態と同じであり、第1実施形態の説明を参照できる。 FIG. 2 is a schematic cross-sectional view of the flexible image display device of the second embodiment. The flexible image display device 101 includes a window member 11, an optical film 12A as the first member, and a laminate of the first laminate L. The first laminated body L has a structure in which an optical film 12B, which is a second member, and a panel member 15B with a second touch sensor, which is a third A member, are laminated. An adhesive member 21 is interposed between the window member 11 and the optical film 12A. An adhesive member 22 is interposed between the optical film 12A and the first laminated body L, and an adhesive member 23 is interposed between the optical film 12B and the panel member 15B with a second touch sensor. Except for the configuration of the optical film 12A and the first laminated body L, which are the first members, the same as the first embodiment, and the description of the first embodiment can be referred to.

光学フィルム12Aは、偏光子121および保護フィルム122で構成される偏光板である。光学フィルム12Aにおいて、偏光子121は、粘着部材22側(換言すると、ウインドウ部材11とは反対側)に配置されている。光学フィルム12Bは、2つの位相差層123および124の積層体である。 The optical film 12A is a polarizing plate composed of a polarizing element 121 and a protective film 122. In the optical film 12A, the polarizer 121 is arranged on the adhesive member 22 side (in other words, the side opposite to the window member 11). The optical film 12B is a laminate of two retardation layers 123 and 124.

第2実施形態については、例えば、第2タッチセンサ付パネル部材15Bを除く構成と図示しないセパレータ(第2セパレータ)との積層体が、光学積層体に相当する。 In the second embodiment, for example, a laminate of a configuration excluding the panel member 15B with a second touch sensor and a separator (second separator) (not shown) corresponds to an optical laminate.

第2実施形態においても、第1実施形態と同様に、E0×T0>0.32(kN/mm)であり、粘着部材21〜23のうち、少なくとも1層の厚みが20μm以上の条件を満たすように制御されている。また、粘着部材21〜23のうち、ウインドウ部材側からn番目の層および(n+1)番目の層の少なくとも一方の厚みが、10μm以上の条件を満たすように、制御されている。そのため、高温環境下でフレキシブル画像表示装置を繰り返し屈曲させても、積層された部材間における高い接着性を確保することができる。また、フレキシブル画像表示装置1および光学積層体のウインドウ部材11側の表面において、比較的高い鉛筆硬度を確保することもできる。 Also in the second embodiment, as in the first embodiment, E0 × T0> 0.32 (kN / mm), and the thickness of at least one layer of the adhesive members 21 to 23 satisfies the condition of 20 μm or more. Is controlled. Further, among the adhesive members 21 to 23, the thickness of at least one of the nth layer and the (n + 1) th layer from the window member side is controlled so as to satisfy the condition of 10 μm or more. Therefore, even if the flexible image display device is repeatedly bent in a high temperature environment, high adhesiveness between the laminated members can be ensured. Further, it is possible to secure a relatively high pencil hardness on the surface of the flexible image display device 1 and the optical laminate on the window member 11 side.

図3は、第3実施形態に係るフレキシブル画像表示装置の概略断面図である。フレキシブル画像表示装置201は、ウインドウ部材11と、第1部材としての光学フィルム12と、第1タッチセンサ付パネル部材15Aとの積層体を備える。ウインドウ部材11と光学フィルム12との間には粘着部材21が介在している。光学フィルム12と第1タッチセンサ付パネル部材15Aとの間には粘着部材22が介在している。第1積層体Lに代えて第1タッチセンサ付パネル部材15Aが配置されている以外は第1実施形態と同じである。第1タッチセンサ付パネル部材15A以外の構成については第1実施形態の説明を参照できる。 FIG. 3 is a schematic cross-sectional view of the flexible image display device according to the third embodiment. The flexible image display device 201 includes a laminated body of a window member 11, an optical film 12 as a first member, and a panel member 15A with a first touch sensor. An adhesive member 21 is interposed between the window member 11 and the optical film 12. An adhesive member 22 is interposed between the optical film 12 and the panel member 15A with the first touch sensor. It is the same as the first embodiment except that the panel member 15A with the first touch sensor is arranged in place of the first laminated body L. For the configurations other than the panel member 15A with the first touch sensor, the description of the first embodiment can be referred to.

第3実施形態については、第1タッチセンサ付パネル部材15Aを除く構成と図示しないセパレータ(第1セパレータ)との積層体が、光学積層体に相当する。 In the third embodiment, the laminated body of the configuration excluding the panel member 15A with the first touch sensor and the separator (first separator) (not shown) corresponds to the optical laminated body.

第3実施形態においても、E0×T0>0.32(kN/mm)であり、粘着部材21および22のうち、少なくとも1層の厚みが20μm以上の条件を満たすように制御されている。また、粘着部材21および22のうち、ウインドウ部材側からn番目の層および(n+1)番目の層の少なくとも一方の厚みが、10μm以上の条件を満たすように、制御されている。そのため、第1および第2実施形態の場合と同様に、積層された部材間における高い接着性を確保することができるとともに、フレキシブル画像表示装置1および光学積層体のウインドウ部材11側の表面において、比較的高い鉛筆硬度を確保することができる。 Also in the third embodiment, E0 × T0> 0.32 (kN / mm), and the thickness of at least one layer of the adhesive members 21 and 22 is controlled so as to satisfy the condition of 20 μm or more. Further, among the adhesive members 21 and 22, the thickness of at least one of the nth layer and the (n + 1) th layer from the window member side is controlled so as to satisfy the condition of 10 μm or more. Therefore, as in the case of the first and second embodiments, high adhesiveness between the laminated members can be ensured, and on the surface of the flexible image display device 1 and the optical laminate on the window member 11 side. A relatively high pencil hardness can be secured.

[実施例]
以下、本発明を実施例および比較例に基づいて具体的に説明するが、本発明は以下の実施例に限定されるものではない。
[Example]
Hereinafter, the present invention will be specifically described based on Examples and Comparative Examples, but the present invention is not limited to the following Examples.

《実施例1〜6、比較例1〜5、および参考例1〜2》
(1)評価用サンプルの作製
図1に示すようなフレキシブル画像表示装置1の評価用サンプルを以下の手順で作製した。
(a)ウインドウ部材11の作製
ウインドウ部材11としては、ウインドウフィルム111としての透明ポリイミドフィルムの片面にアクリル系のハードコート層112(厚み10μm)を設けたものを用いた。ハードコート層112は、ハードコート層用のコーティング剤を用いて形成した。より具体的には、まず、透明ポリイミドフィルムの片面にコーティング剤を塗布して塗布層を形成し、塗布層を透明ポリイミドフィルムとともに90℃で2分間加熱した。次いで、塗布層に高圧水銀ランプを用いて紫外線を積算光量300mJ/cmで照射することによりハードコート層112を形成した。このようにしてウインドウ部材11を作製した。
<< Examples 1 to 6, Comparative Examples 1 to 5, and Reference Examples 1 to 2 >>
(1) Preparation of Evaluation Sample An evaluation sample of the flexible image display device 1 as shown in FIG. 1 was prepared by the following procedure.
(A) Preparation of Window Member 11 As the window member 11, a transparent polyimide film as the window film 111 provided with an acrylic hard coat layer 112 (thickness 10 μm) on one side was used. The hard coat layer 112 was formed by using a coating agent for the hard coat layer. More specifically, first, a coating agent was applied to one side of the transparent polyimide film to form a coating layer, and the coating layer was heated together with the transparent polyimide film at 90 ° C. for 2 minutes. Next, the hard coat layer 112 was formed by irradiating the coating layer with ultraviolet rays using a high-pressure mercury lamp at an integrated light intensity of 300 mJ / cm 2. The window member 11 was manufactured in this way.

ハードコート層用のコーティング剤は、ベース樹脂としての多官能アクリレート(アイカ工業社製、製品名「Z−850−16」)100質量部、レベリング剤(DIC社製、商品名:GRANDIC PC−4100)5質量部、および光重合開始剤(チバ・ジャパン社製、商品名:イルガキュア907)3質量部を混合し、乾燥固形分濃度が50質量%となるように、メチルイソブチルケトンで希釈することにより調製した。 The coating agent for the hard coat layer is 100 parts by mass of a polyfunctional acrylate (manufactured by Aika Kogyo Co., Ltd., product name "Z-850-16") as a base resin, and a leveling agent (manufactured by DIC Co., Ltd., trade name: GRANDIC PC-4100). ) 5 parts by mass and 3 parts by mass of a photopolymerization initiator (manufactured by Ciba Japan, trade name: Irgacure 907) are mixed and diluted with methylisobutylketone so that the dry solid content concentration becomes 50% by mass. Prepared by.

実施例および比較例では、透明ポリイミドフィルムとして、KOLON社製、製品名「A_50_O」、厚み80μmを用いた。既述の手順で求められる実施例および比較例のウインドウ部材の弾性率E0は、4.0GPaであった。実施例および比較例では、E0×T0(=0.09mm)=0.36kN/mmであった。 In Examples and Comparative Examples, a transparent polyimide film manufactured by KOLON, product name "A_50_O", and a thickness of 80 μm was used. The elastic modulus E0 of the window members of the examples and comparative examples obtained by the above-mentioned procedure was 4.0 GPa. In Examples and Comparative Examples, E0 × T0 (= 0.09 mm) = 0.36 kN / mm.

参考例では、透明ポリイミドフィルムとして、KOLON社製、製品名「A_50_O」、厚み50μmを用いた。既述の手順で求められる参考例のウインドウ部材の弾性率E0は、4.7GPaであった。参考例では、E0×T0(=0.06mm)=0.28kN/mmであった。 In the reference example, as the transparent polyimide film, a product name "A_50_O" manufactured by KOLON and a thickness of 50 μm were used. The elastic modulus E0 of the window member of the reference example obtained by the above-mentioned procedure was 4.7 GPa. In the reference example, it was E0 × T0 (= 0.06 mm) = 0.28 kN / mm.

(b)光学フィルム12の作製
下記の手順で光学フィルム12を作製した。
(B) Preparation of Optical Film 12 An optical film 12 was prepared by the following procedure.

(偏光子121の作製)
熱可塑性樹脂製の基材として、イソフタル酸ユニットを7モル%含むアモルファスのポリエチレンテレフタレートフィルム(厚み100μm)を準備し、表面に、58W/m・minの出力放電量でコロナ放電処理を行った。
(Preparation of Polarizer 121)
An amorphous polyethylene terephthalate film (thickness 100 μm) containing 7 mol% of isophthalic acid unit was prepared as a base material made of a thermoplastic resin, and the surface was subjected to corona discharge treatment at an output discharge amount of 58 W / m 2 min. ..

アセトアセチル変性ポリビニルアルコール(日本合成化学工業(株)製、商品名:ゴーセファイマーZ200(平均重合度1200、ケン化度98.5モル%、アセトアセチル化度5モル%))を1質量%添加したポリビニルアルコール(重合度4200、ケン化度99.2%)を準備して、ポリビニルアルコール(PVA)系樹脂を5.5質量%含む水性塗工液を準備した。 1% by mass of acetoacetyl-modified polyvinyl alcohol (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., trade name: Gosefima Z200 (average degree of polymerization 1200, saponification degree 98.5 mol%, acetoacetylation degree 5 mol%)) The added polyvinyl alcohol (degree of polymerization 4200, degree of saponification 99.2%) was prepared, and an aqueous coating liquid containing 5.5% by mass of a polyvinyl alcohol (PVA) -based resin was prepared.

基材の表面に、乾燥後の膜厚が12μmになるように塗工液を塗布し、60℃の雰囲気下、熱風乾燥により10分間乾燥することにより、基材上にPVA系樹脂の層を設けた積層体を作製した。 A coating liquid is applied to the surface of the base material so that the film thickness after drying is 12 μm, and the PVA-based resin layer is formed on the base material by drying in an atmosphere of 60 ° C. for 10 minutes by hot air drying. The provided laminate was produced.

得られた積層体を、まず空気中130℃で1.8倍に自由端延伸(空中補助延伸)することにより、延伸積層体を生成した。次に、延伸積層体を液温30℃のホウ酸不溶化水溶液に30秒間浸漬することにより、延伸積層体に含まれるPVA分子が配向されたPVA層を不溶化する工程を行った。本工程のホウ酸不溶化水溶液は、ホウ酸含有量が水100質量部に対して3質量部であるホウ酸水溶液である。得られた延伸積層体を染色することにより着色積層体を生成した。着色積層体は、延伸積層体を液温30℃のヨウ素およびヨウ化カリウムを含む染色液に、最終的に生成される偏光子を構成するPVA層の単体透過率が40〜44%になるように所定時間、浸漬することで、延伸積層体に含まれるPVA層をヨウ素により染色させたものである。本工程において、染色液は、ヨウ素およびヨウ化カリウムを含む水溶液(ヨウ素濃度:0.1〜0.4質量%、ヨウ化カリウム濃度:0.7〜2.8質量%、ヨウ素とヨウ化カリウムの濃度の比:1対7)である。次に、着色積層体を30℃のホウ酸架橋水溶液に60秒間浸漬することによって、ヨウ素を吸着させたPVA層のPVA分子同士に架橋処理を施す工程を行った。本工程のホウ酸架橋水溶液は、ホウ酸およびヨウ化カリウムを含む水溶液(ホウ酸含有量:水100質量部に対して3質量部、ヨウ化カリウム含有量:水100質量部に対して3質量部)である。 The obtained laminate was first stretched 1.8 times at a free end (auxiliary stretching in the air) at 130 ° C. in the air to produce a stretched laminate. Next, a step of insolubilizing the PVA layer in which the PVA molecules contained in the stretched laminate were oriented was performed by immersing the stretched laminate in a boric acid insoluble aqueous solution having a liquid temperature of 30 ° C. for 30 seconds. The boric acid insoluble aqueous solution in this step is a boric acid aqueous solution having a boric acid content of 3 parts by mass with respect to 100 parts by mass of water. A colored laminate was produced by dyeing the obtained stretched laminate. In the colored laminate, the stretched laminate is mixed with a dyeing solution containing iodine and potassium iodide at a liquid temperature of 30 ° C., and the single transmittance of the PVA layer constituting the polarizer finally produced is 40 to 44%. The PVA layer contained in the stretched laminate was stained with iodine by immersing it in the stretched laminate for a predetermined time. In this step, the staining solution is an aqueous solution containing iodine and potassium iodide (iodine concentration: 0.1-0.4% by mass, potassium iodide concentration: 0.7 to 2.8% by mass, iodine and potassium iodide). Concentration ratio: 1: 7). Next, a step of cross-linking the PVA molecules of the PVA layer on which iodine was adsorbed was performed by immersing the colored laminate in a boric acid cross-linked aqueous solution at 30 ° C. for 60 seconds. The boric acid cross-linked aqueous solution in this step is an aqueous solution containing boric acid and potassium iodide (boric acid content: 3 parts by mass with respect to 100 parts by mass of water, potassium iodide content: 3 parts by mass with respect to 100 parts by mass of water). Department).

得られた着色積層体を、ホウ酸水溶液中、延伸温度70℃で、上記の空気中での延伸と同様の方向に3.05倍に延伸(ホウ酸水中延伸)することにより、最終的な延伸倍率は5.50倍である積層体を得た。得られた積層体をホウ酸水溶液から取り出し、PVA層の表面に付着したホウ酸を、ヨウ化カリウム水溶液(ヨウ化カリウム含有量:水100質量部に対して4質量部)で洗浄した。洗浄された積層体を60℃の温風による乾燥工程により乾燥した。乾燥した積層体に含まれる偏光子121の厚みは5μmであった。 The obtained colored laminate is finally stretched 3.05 times in the boric acid aqueous solution at a stretching temperature of 70 ° C. in the same direction as the above stretching in air (stretching in boric acid water). A laminate having a draw ratio of 5.50 times was obtained. The obtained laminate was taken out from the boric acid aqueous solution, and the boric acid adhering to the surface of the PVA layer was washed with a potassium iodide aqueous solution (potassium iodide content: 4 parts by mass with respect to 100 parts by mass of water). The washed laminate was dried by a drying step with warm air at 60 ° C. The thickness of the polarizer 121 contained in the dried laminate was 5 μm.

(保護フィルム122の形成)
保護フィルム122としては、グルタルイミド環単位を有するメタクリル樹脂ペレットを、押し出し成形により、フィルム状に成形した後、延伸したアクリル系フィルムを用いた。保護フィルムの厚みは40μmであった。保護フィルム122と偏光子121とを接着剤(活性エネルギー線硬化型接着剤)を用いて貼り合わせ、下記の条件で紫外線を照射して接着剤を硬化させることにより偏光板を作製した。
ガリウム封入メタルハライドランプ:Fusion UV Systems.Inc社製、商品名「Light HAMMER10」
バルブ:Vバルブ
ピーク照度:1600mW/cm
積算照射量:1000mJ/cm(波長380〜440nm)
(Formation of protective film 122)
As the protective film 122, an acrylic film obtained by molding a methacrylic resin pellet having a glutarimide ring unit into a film by extrusion molding and then stretching the film was used. The thickness of the protective film was 40 μm. A polarizing plate was produced by bonding the protective film 122 and the polarizer 121 together using an adhesive (active energy ray-curable adhesive) and irradiating the adhesive with ultraviolet rays under the following conditions to cure the adhesive.
Gallium-filled metal halide lamp: Fusion UV Systems. Product name "Light HAMMER10" manufactured by Inc.
Bulb: V bulb Peak illuminance: 1600 mW / cm 2
Integrated irradiation dose: 1000 mJ / cm 2 (wavelength 380 to 440 nm)

接着剤は、下記の成分を接着剤100質量%中の含有量が下記の値となるような割合で混合し、50℃で1時間撹拌することにより調製した。
ヒドロキシエチルアクリルアミド…11.4質量%
トリプロピレングリコールジアクリレート…57.1質量%
アクリロイルモルホリン…11.4質量%
2−アセトアセトキシエチルメタクリレート…4.6質量%
アクリル系ポリマー(ARUFON UP−1190、東亞合成社製)…11.4質量%
2−メチル−1−(4−メチルチオフェニル)−2−モルフォリノプロパン−1−オン…2.8質量%
ジエチルチオキサントン…1.3質量%
The adhesive was prepared by mixing the following components at a ratio such that the content in 100% by mass of the adhesive had the following value, and stirring at 50 ° C. for 1 hour.
Hydroxyethyl acrylamide ... 11.4% by mass
Tripropylene glycol diacrylate ... 57.1% by mass
Acryloyl morpholine ... 11.4% by mass
2-Acetacetoxyethyl methacrylate ... 4.6% by mass
Acrylic polymer (ARUFON UP-1190, manufactured by Toagosei Co., Ltd.) ... 11.4% by mass
2-Methyl-1- (4-methylthiophenyl) -2-morpholinopropane-1-one ... 2.8% by mass
Diethyl thioxanthone ... 1.3% by mass

(位相差層123の作製)
位相差層123としては、液晶材料が配向および固定化された1/4波長板用位相差層と、1/2波長板用位相差層との2層を備える位相差膜を用いた。1/2波長板用位相差層、1/4波長板用位相差層を形成する材料としては、ネマチック液晶相を示す重合性液晶材料(BASF社製・商品名PaliocolorLC242)を用いた。位相差層123は、特開2018−28573号公報の段落[0118]〜[0120]の記載を参照して作製した。
(Preparation of retardation layer 123)
As the retardation layer 123, a retardation film including two layers, a retardation layer for a 1/4 wave plate in which a liquid crystal material is oriented and immobilized, and a retardation layer for a 1/2 wavelength plate was used. As a material for forming the retardation layer for the 1/2 wave plate and the retardation layer for the 1/4 wave plate, a polymerizable liquid crystal material (manufactured by BASF, trade name Pariocolor LC242) showing a nematic liquid crystal phase was used. The retardation layer 123 was prepared with reference to the description in paragraphs [0118] to [0120] of JP-A-2018-288573.

(光学フィルム12の作製)
上記で得られた偏光板と位相差層123とを、上記の接着剤(活性エネルギー線硬化型接着剤)を用いて、ロールツーロール方式により連続的に貼り合わせた。このとき、遅相軸と吸収軸との軸角度が45°となるように積層させた。このようにして光学フィルム12を作製した。既述の手順で求められる光学フィルムの弾性率E1は、4.8GPaであり、E1×T1(=0.05mm)=0.24kN/mmであった。
(Preparation of Optical Film 12)
The polarizing plate obtained above and the retardation layer 123 were continuously bonded by a roll-to-roll method using the above adhesive (active energy ray-curable adhesive). At this time, the layers were laminated so that the axis angle between the slow phase axis and the absorption axis was 45 °. The optical film 12 was produced in this way. The elastic modulus E1 of the optical film obtained by the procedure described above was 4.8 GPa, and E1 × T1 (= 0.05 mm) = 0.24 kN / mm.

(c)加飾層の形成
光学フィルム12のタッチセンサ13側となる表面には、加飾層30として、スクリーン印刷によりフレーム状の黒色インキ層(幅15mm、厚み5μm)を設けた。黒色インキとしては、帝国インキ社製INQ−HF979を用いた。
(C) Formation of Decorative Layer A frame-shaped black ink layer (width 15 mm, thickness 5 μm) was provided as a decorative layer 30 on the surface of the optical film 12 on the touch sensor 13 side by screen printing. As the black ink, INQ-HF979 manufactured by Teikoku Printing Co., Ltd. was used.

(d)粘着剤の調製
粘着部材21〜23を作製するための粘着剤(a1)〜(a3)を下記の手順で調製した。
(D) Preparation of Adhesives Adhesives (a1) to (a3) for producing the adhesive members 21 to 23 were prepared by the following procedure.

(a1)アクリル系粘着剤1:下記の手順で得られるアクリル系粘着剤組成物
(アクリル系ポリマー溶液の調製)
撹拌羽根、温度計、窒素ガス導入管、および冷却器を備えた4つ口フラスコに、ブチルアクリレート99質量部、4−ヒドロキシブチルアクリレート1質量部を含有するモノマー混合物を仕込んだ。このモノマー混合物100質量部に対して、重合開始剤として2,2’−アゾビスイソブチロニトリルを、0.1質量部を酢酸エチルと共に添加した。得られる混合物を緩やかに撹拌しながら窒素ガスを導入して窒素置換を行った。次いで、フラスコ内の液温を55℃付近に保って7時間重合反応を行った。得られた反応液に、酢酸エチルを加えて、ポリマー成分の濃度30質量%に調整した、重量平均分子量160万のアクリル系ポリマーA1の溶液を調製した。
(A1) Acrylic Adhesive 1: An acrylic adhesive composition obtained by the following procedure (preparation of an acrylic polymer solution)
A four-necked flask equipped with a stirring blade, a thermometer, a nitrogen gas introduction tube, and a cooler was charged with a monomer mixture containing 99 parts by mass of butyl acrylate and 1 part by mass of 4-hydroxybutyl acrylate. To 100 parts by mass of this monomer mixture, 2,2'-azobisisobutyronitrile was added as a polymerization initiator, and 0.1 part by mass was added together with ethyl acetate. Nitrogen gas was introduced while gently stirring the obtained mixture to carry out nitrogen substitution. Then, the liquid temperature in the flask was maintained at around 55 ° C., and the polymerization reaction was carried out for 7 hours. Ethyl acetate was added to the obtained reaction solution to prepare a solution of an acrylic polymer A1 having a weight average molecular weight of 1.6 million, which was adjusted to a concentration of a polymer component of 30% by mass.

(アクリル系粘着剤1の調製)
アクリル系ポリマーA1の溶液のポリマー成分100質量部に対して、イソシアネート系架橋剤(商品名:タケネートD110N、トリメチロールプロパンキシリレンジイソシアネート、三井化学(株)製)0.1質量部、過酸化物系架橋剤(ベンゾイルパーオキサイド(商品名:ナイパーBMT、日本油脂(株)製))0.3質量部と、シランカップリング剤(商品名:KBM403、信越化学工業(株)製)0.08質量部とを混合することにより、アクリル系粘着剤1を調製した。
(Preparation of acrylic adhesive 1)
0.1 part by mass of isocyanate-based cross-linking agent (trade name: Takenate D110N, trimethylolpropanexylylene diisocyanate, manufactured by Mitsui Kagaku Co., Ltd.), peroxide with respect to 100 parts by mass of the polymer component of the solution of acrylic polymer A1. 0.3 parts by mass of a cross-linking agent (benzoyl peroxide (trade name: Niper BMT, manufactured by Nippon Yushi Co., Ltd.)) and a silane coupling agent (trade name: KBM403, manufactured by Shin-Etsu Chemical Industry Co., Ltd.) 0.08 The acrylic pressure-sensitive adhesive 1 was prepared by mixing with parts by mass.

(a2)アクリル系粘着剤2:下記の手順で得られるアクリル系粘着剤組成物
(アクリル系ポリマー溶液の調製)
撹拌羽根、温度計、窒素ガス導入管、および冷却器を備えた4つ口フラスコに、ブチルアクリレート94.9質量部、アクリル酸5質量部、および2−ヒドロキシエチルアクリレート0.1質量部を含有するモノマー混合物を仕込んだ。このモノマー混合物の乾燥固形分100質量部に対して、重合開始剤として2,2’−アゾビスイソブチロニトリルを0.1質量部、酢酸エチルと共に添加した。得られる混合物を緩やかに撹拌しながら窒素ガスを導入して窒素置換を行った。次いで、フラスコ内の液温を55℃付近に保って7時間重合反応を行った。得られた反応液に、酢酸エチルを加えて、ポリマー成分の濃度を30質量%に調整した、重量平均分子量200万のアクリル系ポリマーA2の溶液を調製した。
(A2) Acrylic adhesive 2: Acrylic adhesive composition obtained by the following procedure (preparation of an acrylic polymer solution)
A four-necked flask equipped with a stirring blade, a thermometer, a nitrogen gas introduction tube, and a cooler contains 94.9 parts by mass of butyl acrylate, 5 parts by mass of acrylic acid, and 0.1 parts by mass of 2-hydroxyethyl acrylate. A mixture of monomers was charged. To 100 parts by mass of the dry solid content of this monomer mixture, 0.1 parts by mass of 2,2'-azobisisobutyronitrile as a polymerization initiator was added together with ethyl acetate. Nitrogen gas was introduced while gently stirring the obtained mixture to carry out nitrogen substitution. Then, the liquid temperature in the flask was maintained at around 55 ° C., and the polymerization reaction was carried out for 7 hours. Ethyl acetate was added to the obtained reaction solution to prepare a solution of an acrylic polymer A2 having a weight average molecular weight of 2 million, wherein the concentration of the polymer component was adjusted to 30% by mass.

(アクリル系粘着剤2の調製)
アクリル系ポリマーA2の溶液のポリマー成分100質量部に対して、イソシアネート系架橋剤(商品名:コロネートL、トリメチロールプロパントリレンジイソシアネート、日本ポリウレタン工業社製)0.6質量部と、シランカップリング剤(商品名KBM403、信越化学工業(株)製)0.08質量部とを混合することにより、アクリル系粘着剤2を調製した。
(Preparation of acrylic adhesive 2)
With respect to 100 parts by mass of the polymer component of the solution of the acrylic polymer A2, 0.6 parts by mass of an isocyanate-based cross-linking agent (trade name: Coronate L, trimethylolpropane tolylene diisocyanate, manufactured by Nippon Polyurethane Industry Co., Ltd.) and silane coupling An acrylic pressure-sensitive adhesive 2 was prepared by mixing with 0.08 parts by mass of an agent (trade name: KBM403, manufactured by Shin-Etsu Chemical Industry Co., Ltd.).

(a3)アクリル系粘着剤3:下記の手順で得られるアクリル系粘着剤組成物
(アクリル系オリゴマーの調製)
モノマー成分としてメタクリル酸ジシクロペンタニル60質量部およびメタクリル酸メチル40質量部、連鎖移動剤としてα−チオグリセロール3.5質量部、および重合溶媒としてトルエン100質量部を混合し、窒素雰囲気下にて70℃で1時間撹拌した。次に、熱重合開始剤として2,2’−アゾビスイソブチロニトリル0.2質量部を投入し、70℃で2時間反応させた後、80℃に昇温して2時間反応させた。その後、反応液を130℃に加熱して、トルエン、連鎖移動剤および未反応モノマーを乾燥除去して、固形状のアクリル系オリゴマーを得た。アクリル系オリゴマーの重量平均分子量は5100であり、ガラス転移温度(Tg)は130℃であった。
(A3) Acrylic adhesive 3: Acrylic adhesive composition obtained by the following procedure (preparation of acrylic oligomer)
60 parts by mass of dicyclopentanyl methacrylate and 40 parts by mass of methyl methacrylate as a monomer component, 3.5 parts by mass of α-thioglycerol as a chain transfer agent, and 100 parts by mass of toluene as a polymerization solvent are mixed under a nitrogen atmosphere. The mixture was stirred at 70 ° C. for 1 hour. Next, 0.2 parts by mass of 2,2'-azobisisobutyronitrile was added as a thermal polymerization initiator, and the mixture was reacted at 70 ° C. for 2 hours, then heated to 80 ° C. and reacted for 2 hours. .. Then, the reaction solution was heated to 130 ° C., and toluene, the chain transfer agent and the unreacted monomer were dried and removed to obtain a solid acrylic oligomer. The weight average molecular weight of the acrylic oligomer was 5100, and the glass transition temperature (Tg) was 130 ° C.

(プレポリマー組成物の調製)
ラウリルアクリレート43質量部、2−エチルヘキシルアクリレート44質量部、4−ヒドロキシブチルアクリレート6質量部、およびN−ビニル−2−ピロリドン7質量部、ならびに光重合開始剤としてBASF社製「イルガキュア184」0.015質量部を混合し、紫外線を照射して重合を行うことにより、プレポリマー組成物(重合率:約10%)を得た。
(Preparation of prepolymer composition)
43 parts by mass of lauryl acrylate, 44 parts by mass of 2-ethylhexyl acrylate, 6 parts by mass of 4-hydroxybutyl acrylate, and 7 parts by mass of N-vinyl-2-pyrrolidone, and BASF's "Irgacure 184" as a photopolymerization initiator. A prepolymer composition (polymerization rate: about 10%) was obtained by mixing 015 parts by mass and irradiating with ultraviolet rays to carry out polymerization.

(アクリル系粘着剤3の調製)
上記のプレポリマー組成物100質量部に、1,6−ヘキサンジオールジアクリレート0.07質量部、上記のアクリル系オリゴマー1質量部、およびシランカップリング剤(信越化学工業(株)製「KBM403J」)0.3質量部を添加し、均一に混合することにより、アクリル系粘着剤3を調製した。
(Preparation of acrylic adhesive 3)
In addition to 100 parts by mass of the above prepolymer composition, 0.07 parts by mass of 1,6-hexanediol diacrylate, 1 part by mass of the above acrylic oligomer, and a silane coupling agent (“KBM403J” manufactured by Shin-Etsu Chemical Industry Co., Ltd.” ) 0.3 parts by mass was added and mixed uniformly to prepare an acrylic pressure-sensitive adhesive 3.

(e)粘着剤層の形成
上記(d)で調製した粘着剤(表1に示す粘着剤)を用いて、粘着部材21〜23の各層を形成するための粘着剤層を形成した。より具体的には、表1に示す粘着剤を、剥離フィルムにファウンテンコータで均一に塗布し、155℃の空気循環式恒温オーブンで2分間乾燥し、剥離フィルムの表面に粘着剤層を形成した。剥離フィルムとしては、シリコーン系剥離剤で処理された厚さ38μmのポリエチレンテレフタレートフィルム(透明基材、セパレータ)を用いた。粘着剤層の厚みは、サンプルにおける各粘着部材の厚みが表1の値となるように、粘着剤の塗布量によって調節した。
(E) Formation of Adhesive Layer Using the adhesive (adhesive shown in Table 1) prepared in (d) above, an adhesive layer for forming each layer of the adhesive members 21 to 23 was formed. More specifically, the adhesive shown in Table 1 was uniformly applied to the release film with a fountain coater and dried in an air circulation type constant temperature oven at 155 ° C. for 2 minutes to form an adhesive layer on the surface of the release film. .. As the release film, a polyethylene terephthalate film (transparent substrate, separator) having a thickness of 38 μm treated with a silicone-based release agent was used. The thickness of the pressure-sensitive adhesive layer was adjusted by the amount of the pressure-sensitive adhesive applied so that the thickness of each pressure-sensitive adhesive member in the sample had the values shown in Table 1.

(f)積層体の作製
上記で作製した各部材は、必要に応じて、所定のサイズにカットした。各粘着部材を挟持させる部材の一方に、粘着剤層を剥離フィルムから転写し、粘着剤層を挟むように各部材を積層してハンドローラで圧着させた。このようにして、粘着部材により各部材が積層された評価用サンプルを作製した。なお、タッチセンサ13およびパネル部材14としては、それぞれ、透明ポリイミドフィルム(KOLON社製、製品名「A_50_O」、厚み50μm)をダミーとして用いた。なお、既述の手順で求められる透明ポリイミドフィルムの弾性率E2(またはE3)は、6GPaであり、E2(またはE3)×T2(またはT3)=0.3kN/mmであった。
(F) Preparation of Laminated Body Each member produced above was cut into a predetermined size as needed. The pressure-sensitive adhesive layer was transferred from the release film to one of the members holding each pressure-sensitive adhesive member, and each member was laminated so as to sandwich the pressure-sensitive adhesive layer and pressure-bonded by a hand roller. In this way, an evaluation sample in which each member was laminated by the adhesive member was prepared. As the touch sensor 13 and the panel member 14, a transparent polyimide film (manufactured by KOLON, product name "A_50_O", thickness 50 μm) was used as a dummy. The elastic modulus E2 (or E3) of the transparent polyimide film obtained by the procedure described above was 6 GPa, and E2 (or E3) × T2 (or T3) = 0.3 kN / mm.

(2)評価
(a)粘着部材の貯蔵弾性率
各粘着部材の貯蔵弾性率を、既述の手順で求めた。各アクリル系粘着剤を用いた粘着部材の貯蔵弾性率は以下の通りである。
アクリル系粘着剤1(a1)を用いた粘着部材:0.08MPa
アクリル系粘着剤2(a2)を用いた粘着部材:0.12MPa
アクリル系粘着剤3(a3)を用いた粘着部材:0.03MPa
(2) Evaluation (a) Storage elastic modulus of the adhesive member The storage elastic modulus of each adhesive member was determined by the procedure described above. The storage elastic modulus of the pressure-sensitive adhesive member using each acrylic pressure-sensitive adhesive is as follows.
Adhesive member using acrylic adhesive 1 (a1): 0.08 MPa
Adhesive member using acrylic adhesive 2 (a2): 0.12 MPa
Adhesive member using acrylic adhesive 3 (a3): 0.03 MPa

(b)鉛筆硬度試験
評価用サンプルをガラス板上に置き、ウインドウ部材11側の表面(ハードコート層112の表面)における鉛筆硬度を測定した。
(B) Pencil hardness test An evaluation sample was placed on a glass plate, and the pencil hardness on the surface of the window member 11 side (the surface of the hard coat layer 112) was measured.

(c)接着性
上記で得られる評価用サンプルを、偏光板の吸収軸の方向を長辺として、100mm×20mmの短冊状に切り出した。切り出したサンプルを、無負荷U字伸縮試験機(ユアサシステム機器社製「小型卓上型耐久試験機DLMD111LHA」および「U字伸縮試験冶具」)に、ウインドウ部材側を屈曲の内側となるようにセットし、下記の条件で屈曲試験を行った。
環境条件:60℃、55%RH
試験速度:60rpm
屈曲半径:R3
屈曲回数:10万回
(C) Adhesiveness The evaluation sample obtained above was cut into strips of 100 mm × 20 mm with the direction of the absorption axis of the polarizing plate as the long side. Set the cut out sample in a no-load U-shaped expansion / contraction tester (“Small desktop durability tester DLMD111LHA” and “U-shape expansion / contraction test jig” manufactured by Yuasa System Equipment Co., Ltd.) so that the window member side is inside the bend. Then, a bending test was conducted under the following conditions.
Environmental conditions: 60 ° C, 55% RH
Test speed: 60 rpm
Bending radius: R3
Number of bends: 100,000 times

試験後のサンプルの屈曲部分における剥離の状態を目視で観察し、下記の基準で評価した。
A:積層した部材間に剥離が発生していない。
B:積層された部材間に剥離が観察される。
The state of peeling at the bent portion of the sample after the test was visually observed and evaluated according to the following criteria.
A: No peeling has occurred between the laminated members.
B: Peeling is observed between the laminated members.

実施例1〜6、比較例1〜5、および参考例1〜2の結果を表1に示す。これらの表において、e1〜e6は、実施例1〜6であり、c1〜c5は、比較例1〜5であり、r1〜r2は、参考例1〜2である。 The results of Examples 1 to 6, Comparative Examples 1 to 5, and Reference Examples 1 to 2 are shown in Table 1. In these tables, e1 to e6 are Examples 1 to 6, c1 to c5 are Comparative Examples 1 to 5, and r1 to r2 are Reference Examples 1 and 2.

Figure 0006903804
Figure 0006903804

表1に示されるように、E0×T0≦0.32(kN/mm)の場合には、厚みが20μm以上の粘着部材の層を有さない場合および厚みが10μm未満の粘着部材の層が連続する場合でも、高い接着性が得られる(r1およびr2)。ところが、粘着部材の層の厚みがr1およびr2と同じであっても、E0×T0>0.32(kN/mm)の場合には、積層された部材間で剥離が生じる(c3およびc5)。また、表1に示されるように、厚みが比較的大きい(具体的には15μmの)粘着部材の層を複数層有する場合でも、積層された部材間における剥離を抑制することはできない(c1およびc4)。 As shown in Table 1, when E0 × T0 ≦ 0.32 (kN / mm), there is no layer of the adhesive member having a thickness of 20 μm or more, and the layer of the adhesive member having a thickness of less than 10 μm is formed. High adhesiveness is obtained even when continuous (r1 and r2). However, even if the thickness of the layer of the adhesive member is the same as that of r1 and r2, when E0 × T0> 0.32 (kN / mm), peeling occurs between the laminated members (c3 and c5). .. Further, as shown in Table 1, even when a plurality of layers of adhesive members having a relatively large thickness (specifically, 15 μm) are provided, peeling between the laminated members cannot be suppressed (c1 and). c4).

一方、実施例では、複数層の粘着部材の少なくとも1層の厚みを20μm以上とし、ウインドウ部材側からn番目の層および(n+1)番目の層の少なくとも一方の厚みを、10μm以上とする。このような構成により、E0×T0>0.32(kN/mm)の場合でも、高温環境下での屈曲試験において積層された部材間における剥離が見られず、高い接着性を確保できる(e1〜e6)。また、サンプルが10μm未満の小さい厚みの粘着部材の層を含む場合であっても、高い接着性を確保することができる(e1およびe3)。 On the other hand, in the embodiment, the thickness of at least one layer of the plurality of adhesive members is 20 μm or more, and the thickness of at least one of the nth layer and the (n + 1) th layer from the window member side is 10 μm or more. With such a configuration, even when E0 × T0> 0.32 (kN / mm), no peeling is observed between the laminated members in the bending test in a high temperature environment, and high adhesiveness can be ensured (e1). ~ E6). Further, even when the sample contains a layer of an adhesive member having a small thickness of less than 10 μm, high adhesiveness can be ensured (e1 and e3).

いずれの実施例でも、3H以上の高い鉛筆硬度を確保することができている。より高い鉛筆硬度を確保する観点からは、複数層の粘着部材の厚みの平均値は、20μm以下または20μm未満であることが好ましく、19μm以下または18μm以下がより好ましい。同様の観点から、ウインドウ部材側から1番目の層(つまり、粘着部材21)の厚みは、20μm以下または20μm未満が好ましく、17μm以下がより好ましく、16μm以下または15μm以下がさらに好ましい。 In any of the examples, a high pencil hardness of 3H or more can be secured. From the viewpoint of ensuring higher pencil hardness, the average value of the thicknesses of the plurality of layers of the adhesive member is preferably 20 μm or less or less than 20 μm, and more preferably 19 μm or less or 18 μm or less. From the same viewpoint, the thickness of the first layer (that is, the adhesive member 21) from the window member side is preferably 20 μm or less or less than 20 μm, more preferably 17 μm or less, still more preferably 16 μm or less or 15 μm or less.

《実施例7〜12、比較例6〜9、および参考例3〜4》
実施例1〜6に準じて、図3に示すようなフレキシブル画像表示装置201の評価用サンプルを作製した。実施例1のタッチセンサ13およびパネル部材14のダミーの代わりに、第1タッチセンサ付パネル部材15Aのダミーとして、透明ポリイミドフィルム(KOLON社製、製品名「A_50_O」、厚み50μm)をダミーとして用いた。
<< Examples 7 to 12, Comparative Examples 6 to 9, and Reference Examples 3 to 4 >>
An evaluation sample of the flexible image display device 201 as shown in FIG. 3 was prepared according to Examples 1 to 6. Instead dummy of data Tchisensa 13 and panel member 14 of Example 1, use as a dummy of the first touch sensor with the panel member 15A, a transparent polyimide film (KOLON Co., product name "A_50_O", thickness 50 [mu] m) as a dummy There was.

粘着剤層の形成には、実施例1〜6と同様にして調製した粘着剤(表2に示す粘着剤)を用いた。粘着剤層の厚みは、サンプルにおける各粘着部材の厚みが表2の値となるように、粘着剤の塗布量によって調節した。 For the formation of the pressure-sensitive adhesive layer, a pressure-sensitive adhesive (the pressure-sensitive adhesive shown in Table 2) prepared in the same manner as in Examples 1 to 6 was used. The thickness of the pressure-sensitive adhesive layer was adjusted by the amount of the pressure-sensitive adhesive applied so that the thickness of each pressure-sensitive adhesive member in the sample had the values shown in Table 2.

実施例および比較例では、ウインドウ部材として、KOLON社製、製品名「A_50_O」、厚み80μmの透明ポリイミドフィルムを用いた。既述の手順で求められる実施例および比較例のウインドウ部材の弾性率E0は、4.0GPaであった。実施例および比較例では、E0×T0(=0.09mm)=0.36kN/mmであった。 In Examples and Comparative Examples, a transparent polyimide film manufactured by KOLON, product name "A_50_O", and a thickness of 80 μm was used as the window member. The elastic modulus E0 of the window members of the examples and comparative examples obtained by the above-mentioned procedure was 4.0 GPa. In Examples and Comparative Examples, E0 × T0 (= 0.09 mm) = 0.36 kN / mm.

参考例では、ウインドウ部材として、KOLON社製、製品名「A_50_O」、厚み50μmの透明ポリイミドフィルムを用いた。既述の手順で求められる参考例のウインドウ部材の弾性率E0は、4.7GPaであった。参考例では、E0×T0(=0.06mm)=0.28kN/mmであった。 In the reference example, a transparent polyimide film manufactured by KOLON, having a product name of "A_50_O" and a thickness of 50 μm was used as the window member. The elastic modulus E0 of the window member of the reference example obtained by the above-mentioned procedure was 4.7 GPa. In the reference example, it was E0 × T0 (= 0.06 mm) = 0.28 kN / mm.

得られたサンプルを用いて、実施例1〜6と同様にして評価を行った。
実施例7〜12、比較例6〜9、および参考例3〜4の結果を表2に示す。表2において、実施例7〜12は、e7〜e12であり、比較例6〜9は、c6〜c9であり、参考例3〜4は、r3〜r4である。
Using the obtained sample, evaluation was performed in the same manner as in Examples 1 to 6.
The results of Examples 7 to 12, Comparative Examples 6 to 9, and Reference Examples 3 to 4 are shown in Table 2. In Table 2, Examples 7 to 12 are e7 to e12, Comparative Examples 6 to 9 are c6 to c9, and Reference Examples 3 to 4 are r3 to r4.

Figure 0006903804
Figure 0006903804

表2に示されるように、E0×T0≦0.32(kN/mm)の場合には、厚みが20μm以上の粘着部材の層を有さない場合および厚みが10μm未満の粘着部材の層が連続する場合でも、高い接着性が得られる(r4およびr3)。ところが、粘着部材の層の厚みがr3およびr4と同じであっても、E0×T0>0.32(kN/mm)の場合には、積層された部材間で剥離が生じる(c7およびc9)。また、表2に示されるように、厚みが比較的大きい(具体的には15μmの)粘着部材の層を複数層有する場合でも、積層された部材間における剥離を抑制することはできない(c6およびc8)。 As shown in Table 2, when E0 × T0 ≦ 0.32 (kN / mm), there is no layer of the adhesive member having a thickness of 20 μm or more and a layer of the adhesive member having a thickness of less than 10 μm. High adhesiveness is obtained even when continuous (r4 and r3). However, even if the thickness of the layer of the adhesive member is the same as that of r3 and r4, when E0 × T0> 0.32 (kN / mm), peeling occurs between the laminated members (c7 and c9). .. Further, as shown in Table 2, even when a plurality of layers of adhesive members having a relatively large thickness (specifically, 15 μm) are provided, peeling between the laminated members cannot be suppressed (c6 and). c8).

一方、実施例では、複数層の粘着部材の少なくとも1層の厚みを20μm以上とし、ウインドウ部材側からn番目の層および(n+1)番目の層の少なくとも一方の厚みを、10μm以上とする。このような構成により、E0×T0>0.32(kN/mm)の場合でも、高温環境下での屈曲試験において積層された部材間における剥離が見られず、高い接着性を確保できる(e7〜e12)。また、サンプルが10μm未満の小さい厚みの粘着部材の層を含む場合であっても、高い接着性を確保することができる(e7およびe9)。 On the other hand, in the embodiment, the thickness of at least one layer of the plurality of adhesive members is 20 μm or more, and the thickness of at least one of the nth layer and the (n + 1) th layer from the window member side is 10 μm or more. With such a configuration, even when E0 × T0> 0.32 (kN / mm), no peeling is observed between the laminated members in the bending test in a high temperature environment, and high adhesiveness can be ensured (e7). ~ E12). Further, even when the sample contains a layer of an adhesive member having a small thickness of less than 10 μm, high adhesiveness can be ensured (e7 and e9).

いずれの実施例でも、3H以上の高い鉛筆硬度を確保することができている。より高い鉛筆硬度を確保する観点からは、ウインドウ部材側から1番目の粘着部材の層の厚みは、20μm以下であり、複数層の粘着部材の厚みの平均値は、20μm以下であることが好ましい。 In any of the examples, a high pencil hardness of 3H or more can be secured. From the viewpoint of ensuring higher pencil hardness, the thickness of the first adhesive member layer from the window member side is preferably 20 μm or less, and the average value of the thicknesses of the plurality of adhesive members is preferably 20 μm or less. ..

1、101、201:フレキシブル画像表示装置
11:ウインドウ部材
111:ウインドウフィルム
112:ハードコート層
12、12A、12B:光学フィルム
121:偏光子
122:保護フィルム
123、124:位相差層
13:タッチセンサ
131:透明導電層
132:透明フィルム
14:パネル部材
141:有機ELパネル
142:薄膜封止層
15A:第1タッチセンサ付パネル部材
15B:第2タッチセンサ付パネル部材
L:第1積層体
21、22、23:粘着部材
30:加飾層
1, 101, 201: Flexible image display device 11: Window member 111: Window film 112: Hard coat layer 12, 12A, 12B: Optical film 121: Polarizer 122: Protective film 123, 124: Phase difference layer 13: Touch sensor 131: Transparent conductive layer 132: Transparent film 14: Panel member 141: Organic EL panel 142: Thin film sealing layer 15A: Panel member with first touch sensor 15B: Panel member with second touch sensor L: First laminated body 21, 22, 23 : Adhesive member 30: Decorative layer

Claims (14)

透明樹脂フィルムを備えたウインドウ部材と、
前記ウインドウ部材に積層された第1部材と、
前記ウインドウ部材に前記第1部材を介して積層された第1積層体または第1タッチセンサ付パネル部材と、
複数層の粘着部材と、を具備するフレキシブル画像表示装置であって、
前記第1積層体は、前記ウインドウ部材に、前記第1部材を介して積層された第2部材と、前記第1部材および前記第2部材を介して積層された第3A部材との積層体であり、
前記フレキシブル画像表示装置が前記第1積層体を備える場合、
前記第1部材および前記第2部材の一方は、光学フィルムであり、他方は、光学フィルムまたはタッチセンサであり、
前記第3A部材は、少なくともパネル部材を含み、
前記複数層の粘着部材は、少なくとも、前記ウインドウ部材と前記第1部材との間、前記第1部材と前記第2部材との間、および前記第2部材と前記第3A部材との間に配置される3層を含み、
前記フレキシブル画像表示装置が前記第1タッチセンサ付パネル部材を備える場合、
前記第1部材は、光学フィルムであり、
前記複数層の粘着部材は、少なくとも、前記ウインドウ部材と前記第1部材との間、および前記第1部材と前記第1タッチセンサ付パネル部材との間に配置される2層を含み、
前記ウインドウ部材の弾性率(GPa)をE0とし、前記ウインドウ部材の厚み(mm)をT0とするとき、E0×T0(kN/mm)は、E0×T0>0.32の条件を満たし、
前記複数層の粘着部材の少なくとも1層の厚みは、20μm以上の条件を満たし、
前記複数層の粘着部材のうち、前記ウインドウ部材側からn番目の層および(n+1)番目の層の少なくとも一方の厚みは、10μm以上の条件を満たす、フレキシブル画像表示装置。
A window member with a transparent resin film and
The first member laminated on the window member and
A first laminated body or a panel member with a first touch sensor laminated on the window member via the first member.
A flexible image display device including a plurality of layers of adhesive members.
The first laminated body is a laminated body of a second member laminated via the first member and a third A member laminated via the first member and the second member on the window member. Yes,
When the flexible image display device includes the first laminated body,
One of the first member and the second member is an optical film, and the other is an optical film or a touch sensor.
The third A member includes at least a panel member.
The plurality of layers of the adhesive member are arranged at least between the window member and the first member, between the first member and the second member, and between the second member and the third A member. Including 3 layers to be
When the flexible image display device includes the panel member with the first touch sensor,
The first member is an optical film and
The plurality of layers of the adhesive member includes at least two layers arranged between the window member and the first member and between the first member and the panel member with the first touch sensor.
When the elastic modulus (GPa) of the window member is E0 and the thickness (mm) of the window member is T0, E0 × T0 (kN / mm) satisfies the condition of E0 × T0> 0.32.
The thickness of at least one layer of the plurality of adhesive members satisfies the condition of 20 μm or more.
A flexible image display device in which the thickness of at least one of the nth layer and the (n + 1) th layer from the window member side of the plurality of layers of the adhesive member satisfies a condition of 10 μm or more.
前記第3A部材を備え、
前記第1部材および前記第2部材の一方は、前記光学フィルムであり、他方は、前記タッチセンサである、請求項1に記載のフレキシブル画像表示装置。
The third A member is provided.
The flexible image display device according to claim 1, wherein one of the first member and the second member is the optical film, and the other is the touch sensor.
前記複数層の粘着部材は、前記第3A部材内に配置される少なくとも1層をさらに含む、請求項1または2に記載のフレキシブル画像表示装置。 The flexible image display device according to claim 1 or 2, wherein the plurality of layers of the adhesive member further includes at least one layer arranged in the third A member. 前記第3A部材は、第2タッチセンサ付パネル部材を含み、
前記第1部材および前記第2部材のそれぞれは、前記光学フィルムである、請求項1に記載のフレキシブル画像表示装置。
The third A member includes a panel member with a second touch sensor.
The flexible image display device according to claim 1, wherein each of the first member and the second member is the optical film.
前記複数層の粘着部材の厚みの最大値は、50μm以下の条件を満たす、請求項1〜4のいずれか1項に記載のフレキシブル画像表示装置。 The flexible image display device according to any one of claims 1 to 4, wherein the maximum value of the thickness of the plurality of layers of the adhesive member satisfies the condition of 50 μm or less. 前記複数層の粘着部材のうち、前記ウインドウ部材側から1番目の層の厚みは、20μm以下の条件を満たし、
前記複数層の粘着部材の厚みの平均値は、20μm以下の条件を満たす、請求項1〜5のいずれか1項に記載のフレキシブル画像表示装置。
Among the plurality of layers of the adhesive member, the thickness of the first layer from the window member side satisfies the condition of 20 μm or less.
The flexible image display device according to any one of claims 1 to 5, wherein the average value of the thicknesses of the plurality of layers of the adhesive member satisfies the condition of 20 μm or less.
前記複数層の粘着部材の各層の25℃における貯蔵弾性率は、1MPa以下の条件を満たす、請求項1〜6のいずれか1項に記載のフレキシブル画像表示装置。 The flexible image display device according to any one of claims 1 to 6, wherein the storage elastic modulus of each layer of the plurality of layers of the adhesive member at 25 ° C. satisfies the condition of 1 MPa or less. 前記複数層の粘着部材の各層の厚みは、3μm以上の条件を満たす、請求項1〜7のいずれか1項に記載のフレキシブル画像表示装置。 The flexible image display device according to any one of claims 1 to 7, wherein the thickness of each layer of the plurality of layers of the adhesive member satisfies the condition of 3 μm or more. E0×T0は、前記ウインドウ部材側の表面におけるJIS K 5600−5−4:1999に規定される鉛筆硬度を規制する、請求項1〜8のいずれか1項に記載のフレキシブル画像表示装置。 The flexible image display device according to any one of claims 1 to 8, wherein E0 × T0 regulates the pencil hardness specified in JIS K 5600-5-4: 1999 on the surface on the window member side. 前記ウインドウ部材側のJIS K 5600−5−4:1999に規定される鉛筆硬度試験による硬度が、H以上である、請求項1〜のいずれか1項に記載のフレキシブル画像表示装置。 The flexible image display device according to any one of claims 1 to 9 , wherein the hardness according to the pencil hardness test specified in JIS K 5600-5-4: 1999 on the window member side is H or more. 前記ウインドウ部材は、ハードコート層を備え、
前記ハードコート層は、少なくとも前記ウインドウ部材の前記第1部材側とは反対側に設けられている、請求項1〜10のいずれか1項に記載のフレキシブル画像表示装置。
The window member includes a hard coat layer and has a hard coat layer.
The flexible image display device according to any one of claims 1 to 10 , wherein the hard coat layer is provided at least on the side of the window member opposite to the first member side.
前記ウインドウ部材の弾性率E0が、0.53GPa以上16GPa以下である、請求項1〜11のいずれか1項に記載のフレキシブル画像表示装置。The flexible image display device according to any one of claims 1 to 11, wherein the elastic modulus E0 of the window member is 0.53 GPa or more and 16 GPa or less. 請求項1〜12のいずれか1項に記載のフレキシブル画像表示装置に用いられ、
透明樹脂フィルムを備えたウインドウ部材と、
前記ウインドウ部材に積層された第1部材と、
前記ウインドウ部材に前記第1部材を介して積層された第2積層体または第1セパレータと、
複数層の粘着部材と、を具備する光学積層体であって、
前記第2積層体は、前記ウインドウ部材に、前記第1部材を介して積層された第2部材と、前記第1部材および前記第2部材を介して積層された第3B部材との積層体であり、
前記光学積層体が前記第2積層体を備える場合、
前記第1部材および前記第2部材の一方は、光学フィルムであり、他方は、光学フィルムまたはタッチセンサであり、
前記第3B部材は、少なくとも第2セパレータを含み、
前記複数層の粘着部材は、少なくとも、前記ウインドウ部材と前記第1部材との間、前記第1部材と前記第2部材との間、および前記第2部材と前記第3B部材との間に配置される3層を含み、
前記光学積層体が前記第1セパレータを備える場合、
前記第1部材は、光学フィルムであり、
前記複数層の粘着部材は、少なくとも、前記ウインドウ部材と前記第1部材との間、および前記第1部材と前記第1セパレータとの間に配置される2層を含み、
前記ウインドウ部材の弾性率(GPa)をE0とし、前記ウインドウ部材の厚み(mm)をT0とするとき、E0×T0(kN/mm)は、E0×T0>0.32の条件を満たし、
前記複数層の粘着部材の少なくとも1層の厚みは、20μm以上の条件を満たし、
前記複数層の粘着部材のうち、前記ウインドウ部材側からn番目の層および(n+1)番目の層の少なくとも一方の厚みは、10μm以上の条件を満たす、光学積層体。
Used in the flexible image display device according to any one of claims 1 to 12.
A window member with a transparent resin film and
The first member laminated on the window member and
A second laminated body or a first separator laminated on the window member via the first member,
An optical laminate comprising a plurality of layers of adhesive members.
The second laminated body is a laminated body of a second member laminated via the first member and a third B member laminated via the first member and the second member on the window member. Yes,
When the optical laminate includes the second laminate,
One of the first member and the second member is an optical film, and the other is an optical film or a touch sensor.
The third B member includes at least a second separator.
The plurality of layers of the adhesive member are arranged at least between the window member and the first member, between the first member and the second member, and between the second member and the third B member. Including 3 layers to be
When the optical laminate includes the first separator
The first member is an optical film and
The plurality of layers of the adhesive member includes at least two layers arranged between the window member and the first member and between the first member and the first separator.
When the elastic modulus (GPa) of the window member is E0 and the thickness (mm) of the window member is T0, E0 × T0 (kN / mm) satisfies the condition of E0 × T0> 0.32.
The thickness of at least one layer of the plurality of adhesive members satisfies the condition of 20 μm or more.
An optical laminate in which the thickness of at least one of the nth layer and the (n + 1) th layer from the window member side of the plurality of layers of the adhesive member satisfies the condition of 10 μm or more.
前記第3B部材を備え、
前記第1部材および前記第2部材の一方は、前記光学フィルムであり、他方は、前記タッチセンサである、請求項13に記載の光学積層体。
The third B member is provided, and the third B member is provided.
The optical laminate according to claim 13 , wherein one of the first member and the second member is the optical film, and the other is the touch sensor.
JP2020159585A 2019-12-27 2020-09-24 Flexible image display device and optical laminate used for it Active JP6903804B1 (en)