JP6900692B2 - Joining method using rivets and equipment used for its implementation - Google Patents

Joining method using rivets and equipment used for its implementation Download PDF

Info

Publication number
JP6900692B2
JP6900692B2 JP2017020504A JP2017020504A JP6900692B2 JP 6900692 B2 JP6900692 B2 JP 6900692B2 JP 2017020504 A JP2017020504 A JP 2017020504A JP 2017020504 A JP2017020504 A JP 2017020504A JP 6900692 B2 JP6900692 B2 JP 6900692B2
Authority
JP
Japan
Prior art keywords
rivet
punch
die
steel
plate
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
JP2017020504A
Other languages
Japanese (ja)
Other versions
JP2018126752A (en
Inventor
古迫 誠司
誠司 古迫
岡田 徹
徹 岡田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nippon Steel Corp
Original Assignee
Nippon Steel Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nippon Steel Corp filed Critical Nippon Steel Corp
Priority to JP2017020504A priority Critical patent/JP6900692B2/en
Publication of JP2018126752A publication Critical patent/JP2018126752A/en
Application granted granted Critical
Publication of JP6900692B2 publication Critical patent/JP6900692B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Description

本発明は、リベットを用いた接合方法と装置に関し、特に、引張強度が780MPa以上の高強度鋼板を1枚以上含む複数枚の鋼板を接合する方法と装置に関するものである。 The present invention relates to a joining method and apparatus using rivets, and more particularly to a method and apparatus for joining a plurality of steel plates including one or more high-strength steel plates having a tensile strength of 780 MPa or more.

従来、自動車分野では、車体の組立や部品の取付けなどにスポット溶接が多用されており、高強度鋼板を含む複数枚の鋼板の接合などもスポット溶接で行われる。
しかし、引張強度が780MPa以上の鋼板を含むようなスポット溶接継手では、ナゲットの靭性が低下し、剥離方向の応力ではナゲット端部に応力が集中するため、鋼板の引張強さが増加しても、十字引張強さ(CTS)が、増加しないか、又は、減少するという問題がある。
Conventionally, in the automobile field, spot welding is often used for assembling car bodies and attaching parts, and joining of a plurality of steel plates including high-strength steel plates is also performed by spot welding.
However, in a spot-welded joint containing a steel plate having a tensile strength of 780 MPa or more, the toughness of the nugget decreases, and the stress in the peeling direction concentrates the stress on the nugget end, so that even if the tensile strength of the steel plate increases. , There is a problem that the cross tensile strength (CTS) does not increase or decreases.

この問題を解決する技術の一つとして、母材を溶融させることなく機械的に接合する技術、すなわち、被接合材である複数枚の金属板を重ね合わせ、金属板を板押えで押さえながら、パンチでリベットを打ち込み、複数枚の金属板をリベットで接合する技術がある。
しかし、この技術では、リベットを打ち込むため、パンチと接触する金属板と反対側(ダイ側)の金属板の変形が非常に大きくなり、ダイ側の金属板で割れが発生するという問題、せん断方向及び剥離方向に引張応力がかかった場合、リベットが抜けて破壊が生じ、せん断方向及び剥離方向の引張強度で十分な値が得られないという問題などがあった。
As one of the technologies to solve this problem, a technique of mechanically joining without melting the base material, that is, a technique of superimposing a plurality of metal plates to be joined and pressing the metal plates with a plate presser while holding the metal plates together. There is a technology to drive rivets with a punch and join multiple metal plates with rivets.
However, in this technology, since the rivet is driven, the deformation of the metal plate on the opposite side (die side) to the metal plate in contact with the punch becomes very large, and the metal plate on the die side cracks. In addition, when tensile stress is applied in the peeling direction, the rivet comes off and fracture occurs, and there is a problem that sufficient values cannot be obtained in the tensile strength in the shearing direction and the peeling direction.

このような問題を解決する技術として、特許文献1には、最初に、リベット打ち機を通して、高強度鋼板を含む鋼板2、3をセルフピアシング型のリベット7によって機械的に接合し(図7a参照)、次に、スポット溶接機を通して、リベットを含む接合個所を加熱・加圧して、該個所に冶金的に接合された溶接スポット微細構造を形成する(図7b参照)技術が開示されている。 As a technique for solving such a problem, in Patent Document 1, first, steel plates 2 and 3 including high-strength steel plates are mechanically joined by a self-piercing type rivet 7 through a riveting machine (see FIG. 7a). ), Next, a technique is disclosed in which a joint portion including a rivet is heated and pressurized through a spot welder to form a welded spot microstructure metallurgically bonded to the portion (see FIG. 7b).

また、特許文献2には、鉄系金属板3とアルミ系金属板2との異種金属接合方法において、アルミ系金属板側から、鉄系金属製のリベット7を電極で加圧しながら押し込み、リベット7でアルミ系金属板2を貫いて、リベットの先端部7cを鉄系金属板3に接触させ(図8a参照)、電極でリベット7と鉄系金属板3を加圧しながらリベット7と鉄系金属板3との間で通電することにより、リベットの先端部7cと鉄系金属板3を抵抗溶接し(図8b参照)、リベットを介して鉄系金属板とアルミ系金属板を接合する技術が開示されている。 Further, in Patent Document 2, in the method of joining dissimilar metals between the iron-based metal plate 3 and the aluminum-based metal plate 2, the iron-based metal rivet 7 is pushed in while being pressed by an electrode from the aluminum-based metal plate side, and the rivet is rivet. The aluminum metal plate 2 is pierced by No. 7, the tip portion 7c of the rivet is brought into contact with the iron metal plate 3 (see FIG. 8a), and the rivet 7 and the iron metal plate 3 are pressed by the electrodes while the rivet 7 and the iron metal plate 3 are pressed. A technique of resistance-welding the tip 7c of a rivet and an iron-based metal plate 3 by energizing between the metal plate 3 (see FIG. 8b) and joining the iron-based metal plate and the aluminum-based metal plate via the rivet. Is disclosed.

特表2007−521964号公報Special Table 2007-521964 特許第2954476号公報Japanese Patent No. 29544476

特許文献1、2の技術は、スポット溶接及びリベット接合の有する問題点を解決しようとするものであるが、特許文献1の技術では、リベットの打ち込みと抵抗溶接の工程が2工程になるという問題がある。また、特許文献2では、ピンの打ち込みと抵抗溶接を1つの工程で連続的に行っているが、アルミ系金属板を含む継手の溶接に有効な技術であり、少なくとも、鋼板のみを用いた場合の溶接については考慮されていない。 The techniques of Patent Documents 1 and 2 attempt to solve the problems of spot welding and rivet joining, but the technique of Patent Document 1 has a problem that the steps of rivet driving and resistance welding are two steps. There is. Further, in Patent Document 2, pin driving and resistance welding are continuously performed in one step, but this is an effective technique for welding a joint including an aluminum-based metal plate, and at least when only a steel plate is used. Welding is not considered.

そこで、本発明は、引張強さが780MPa以上の高強度鋼板を用いて剥離強度が十分に高い継手を形成することできる接合方法及びその装置を提供することを課題とする。 Therefore, an object of the present invention is to provide a joining method and an apparatus thereof capable of forming a joint having a sufficiently high peel strength by using a high-strength steel plate having a tensile strength of 780 MPa or more.

本発明では、そのような課題に対して、通電加熱を利用したセルフピアシング型の先端部が尖った中実のリベットによる接合と通電加熱による溶融接合(あるいは固相接合)を組み合わせて連続的に一つの工程で行うことによって上記課題を解決した。
そのような本発明の要旨は、以下のとおりである。
In the present invention, in order to solve such a problem, a self-piercing type using energization heating is continuously combined with a solid rivet bonding with a sharp tip and a fusion bonding (or solid phase bonding) by energization heating. The above problem was solved by performing it in one step.
The gist of such an invention is as follows.

(1) 引張強さが780MPa以上の高強度鋼板を少なくとも1枚は含む重ね合わせた複数枚の鋼板をセルフピアシングリベット、ポンチ及びダイを用いて接合する方法であって、
前記ポンチで、前記ポンチの外側にポンチと同軸に配置された板押えで鋼板を加圧しながら前記板押えと前記ダイ間に通電して、鋼板を予備的に加熱した後、
前記リベットとして、鋼よりなり先端部が尖った中実のリベットを用い、ポンチで前記リベットを加圧しながらリベットと前記ダイ間に通電して、前記接合しようとする鋼板を加熱しながら前記鋼板の厚み方向の所定の位置までリベットを押し込み、さらにポンチでリベットを加圧しながら通電を継続して、少なくとも鋼板間を固相接合あるいは溶融接合することを特徴とする接合方法。
(1) A method of joining a plurality of stacked steel sheets including at least one high-strength steel sheet having a tensile strength of 780 MPa or more by using a self-piercing rivet, a punch and a die.
After the steel plate is preheated by energizing between the plate retainer and the die while pressurizing the steel plate with the punch, which is arranged coaxially with the punch on the outside of the punch.
As the rivet, with a solid rivet having a sharp tip made of steel, by energizing between the rivet while pressing the rivet with punch die, of the steel sheet while heating the steel sheet to be the joint A joining method characterized in that a rivet is pushed to a predetermined position in the thickness direction, and then energization is continued while pressurizing the rivet with a punch to perform solid-phase bonding or melt-bonding at least between steel sheets.

) 前記リベットとして、C:0.15質量%以下の鋼を用いることを特徴とする上記(1)に記載の接合方法。
(3) 前記ポンチで前記リベットを加圧しながら前記リベットと前記ダイ間に通電する工程において、
第一電流及び第一加圧力で通電加圧した後、第一電流よりも高い第二電流、及び、第一加圧力よりも高い第二加圧力で通電加圧することを特徴とする上記(1)又は(2)に記載の接合方法。
( 2 ) The joining method according to (1) above, wherein steel having a C: 0.15% by mass or less is used as the rivet.
(3) In the step of energizing between the rivet and the die while pressurizing the rivet with the punch.
After energizing and pressurizing with the first current and the first pressurizing, the energizing and pressurizing is performed with a second current higher than the first current and a second pressurizing higher than the first pressurizing (1). ) Or (2).

(4) 上記(1)に記載の接合方法の実施に使用する接合装置であって、
一方の側に、ポンチと、該ポンチの外側にポンチと同軸に設けられた筒状の板押えを有し、他方の側に、接合しようとする鋼板をポンチに対向して支持するダイを有し、
前記板押えとダイ、前記ポンチとダイがそれぞれ電源装置に接続され、
前記板押えが鋼板と接触した時に板押えとダイ間が通電して鋼板を予備的に加熱した後、前記リベットが鋼板と接触した時に前記ポンチとダイ間が通電して鋼板を加熱するように構成されていることを特徴とする接合装置。
(4) A joining device used to carry out the joining method described in (1) above.
One side has a punch and a tubular plate retainer coaxially provided on the outside of the punch, and the other side has a die that supports the steel plate to be joined facing the punch. And
The plate retainer and die, and the punch and die are connected to the power supply device, respectively.
When the plate retainer comes into contact with the steel plate, the plate retainer and the die are energized to preheat the steel plate, and then when the rivet comes into contact with the steel plate, the punch and the die are energized to heat the steel plate. A joining device characterized by being configured.

(5) 上記(3)に記載の接合方法の実施に使用する接合装置であって、
一方の側に、ポンチと、該ポンチの外側にポンチと同軸に設けられた筒状の板押えを有し、他方の側に、接合しようとする鋼板をポンチに対向して支持するダイを有し、
前記板押えとダイ、前記ポンチとダイがそれぞれ電源装置に接続され、
前記板押えが鋼板と接触した時に板押えとダイ間が通電して鋼板を予備的に加熱した後、
前記リベットが鋼板と接触した時に前記ポンチとダイ間が通電して鋼板をさらに加熱するように構成され、かつ、
前記ポンチとダイ間が通電して鋼板をさらに加熱する際に、第一電流及び第一加圧力で通電加圧した後、第一電流よりも高い第二電流、及び、第一加圧力よりも高い第二加圧力で通電加圧するように構成されていることを特徴とする接合装置。
(5) A joining device used to carry out the joining method described in (3) above.
One side has a punch and a tubular plate retainer coaxially provided on the outside of the punch, and the other side has a die that supports the steel plate to be joined facing the punch. And
The plate retainer and die, and the punch and die are connected to the power supply device, respectively.
When the plate retainer comes into contact with the steel plate, the plate retainer and the die are energized to preheat the steel plate, and then
When the rivet comes into contact with the steel sheet, the punch and the die are energized to further heat the steel sheet, and
When the punch and the die are energized to further heat the steel sheet, after energizing and pressurizing with the first current and the first pressing force, the second current higher than the first current and the first pressing force A joining device characterized in that it is configured to be energized and pressurized with a high second pressing force.

本発明によれば、リベットによる機械的接合と熱を利用した冶金的接合の両方を利用して鋼板を接合するので、高強度鋼板を用いて剥離強度が十分に高い継手を形成することができる。
また、通電加熱を利用するので、高強度鋼板を用いていてもリベットの打ち込みが容易となり、先の尖ったリベットを利用するので加熱に高い電流を必要とせず、接合に要する時間も十分に短くできる。
さらに、リベットに炭素量の低い鋼を用いることにより、接合部のじん性を向上させ、遅れ破壊を抑制することもできる。
According to the present invention, since the steel sheets are joined by using both mechanical joining by rivets and metallurgical joining using heat, it is possible to form a joint having sufficiently high peel strength by using a high-strength steel sheet. ..
In addition, since energization heating is used, it is easy to drive rivets even if a high-strength steel plate is used, and since a pointed rivet is used, a high current is not required for heating and the time required for joining is sufficiently short. it can.
Further, by using steel having a low carbon content for the rivet, the toughness of the joint can be improved and delayed fracture can be suppressed.

本発明の接合方法で用いる装置の概略図である。It is the schematic of the apparatus used in the joining method of this invention. 本発明の接合方法の手順の一例を示す概略図である。It is the schematic which shows an example of the procedure of the joining method of this invention. リベットの形状の一例を示す図である。It is a figure which shows an example of the shape of a rivet. ダイセットの別の態様を示す図である。It is a figure which shows another aspect of the die set. 本発明の方法の実施に使用する装置の概略図である。It is the schematic of the apparatus used for carrying out the method of this invention. 本発明の接合方法で用いる加圧力と電流のパターンの一例を示す図である。It is a figure which shows an example of the pattern of the pressing force and the electric current used in the joining method of this invention. 従来技術を説明するための図である。It is a figure for demonstrating the prior art. 他の従来技術を説明するための図である。It is a figure for demonstrating another prior art.

本発明は、セルフピアシング型のリベットの通電加熱を利用した打ち込みによる接合と通電加熱による溶融接合(あるいは固相接合)を組み合わせて連続的に一つの工程で行うことにより、高強度鋼板を用いて継手強度の高い接合製品を製造することができる。
最初に、本発明の基本的な実施の形態について図面を用いて説明する。
The present invention uses a high-strength steel plate by continuously performing joining by driving using energization heating of a self-piercing type rivet and melt joining (or solid-phase joining) by energization heating in one step. It is possible to manufacture a joint product with high joint strength.
First, a basic embodiment of the present invention will be described with reference to the drawings.

本発明の実施には、図1に概略を示す、互いに対向する一方の側に、ポンチ4と該ポンチの外側にポンチと同軸に設けられた円筒状の板押え5を配置し、他方の側に、接合しようとする鋼板2、3(以下単に鋼板と記載する場合がある)をポンチに対向して支持するダイセット6を有する接合装置1を用いる。なお、ダイセット6は、リベット7に対向するダイ6aと板押え5に対向する押え部6bよりなる。
また、鋼板に打ち込むリベット7は、図3に示すように、一般的なリベットと同様に軸部7aとつば部を有する頭部7bよりなるもので、鋼製で、中実であり、リベットの先端部、すなわち軸部7aの先端7cは釘状に尖っている。
In carrying out the present invention, the punch 4 and the cylindrical plate retainer 5 provided coaxially with the punch are arranged on one side facing each other, which is outlined in FIG. 1, and the other side. A joining device 1 having a die set 6 for supporting the steel plates 2 and 3 to be joined (hereinafter, may be simply referred to as steel plates) facing the punch is used. The die set 6 includes a die 6a facing the rivet 7 and a pressing portion 6b facing the plate pressing 5.
Further, as shown in FIG. 3, the rivet 7 to be driven into the steel plate is composed of a shaft portion 7a and a head portion 7b having a brim portion like a general rivet, is made of steel, is solid, and is a rivet. The tip portion, that is, the tip portion 7c of the shaft portion 7a is pointed like a nail.

ポンチ4とダイ6aは、通電可能な材料で形成され、ともに電源装置8に接続されており、ポンチとダイが鋼板に接触することにより、電気回路が形成されるようになっている。板押え5は、鋼板と接触しても電流が流れないように他の部材と電気的に絶縁されている。 The punch 4 and the die 6a are made of a material that can be energized and are both connected to the power supply device 8. When the punch and the die come into contact with the steel plate, an electric circuit is formed. The plate retainer 5 is electrically insulated from other members so that a current does not flow even if it comes into contact with the steel plate.

図1では、ダイ側が上方で、ポンチ側が下方に配置される例を示すが、ダイ側が下方で、ポンチ側が上方に配置されるものでもよい。 FIG. 1 shows an example in which the die side is arranged on the upper side and the punch side is arranged on the lower side, but the die side may be arranged on the lower side and the punch side may be arranged on the upper side.

以上のような装置を用いて次の手順で接合を行う。
接合しようとする鋼板2、3を重ね合わせて、接合装置1のダイセット6と板押え5間に搬入し、板押え5上に載置する(図1参照)。リベット7は、予めポンチ4上にセットされている。
鋼板2、3としては引張強さが780MPa以上の高強度鋼板を1枚以上含むものとする。重ね合わせる鋼板の枚数は、図1では2枚としているが、3〜5枚程度とすることができる。
Joining is performed by the following procedure using the above device.
The steel plates 2 and 3 to be joined are overlapped, carried between the die set 6 of the joining device 1 and the plate retainer 5, and placed on the plate retainer 5 (see FIG. 1). The rivet 7 is set on the punch 4 in advance.
The steel plates 2 and 3 include one or more high-strength steel plates having a tensile strength of 780 MPa or more. The number of steel plates to be stacked is two in FIG. 1, but it can be about 3 to 5.

次に、ダイセット6を鋼板側に移動させて、鋼板をダイセット6と板押え5で挟んで、鋼板を保持した後(図2a参照)、ポンチ4を板押え5を通して鋼板側に移動させ、ポンチ先端に位置するリベット7を鋼板側に押出し、リベット先端7cを鋼板2に接触させ(図2b参照)、さらにポンチ4でリベット7を加圧して、その先端部を鋼板2に食い込ませる(図2c参照)。 Next, the die set 6 is moved to the steel plate side, the steel plate is sandwiched between the die set 6 and the plate retainer 5 to hold the steel plate (see FIG. 2a), and then the punch 4 is moved to the steel plate side through the plate retainer 5. , The rivet 7 located at the tip of the punch is extruded toward the steel plate, the tip 7c of the rivet is brought into contact with the steel plate 2 (see FIG. 2b), and the rivet 7 is further pressed by the punch 4 so that the tip bites into the steel plate 2 (see FIG. 2b). See FIG. 2c).

その際、リベットの先端7cが鋼板2に接触した後、ポンチ4とダイ6a間に通電することにより、リベット先端と鋼板に電流が流れ、リベットと鋼板が通電加熱される。
リベット先端7cは尖っているため、通電中にリベットの先端とそれに接触する鋼板に電流と応力が集中し、鋼板の温度が急激に上昇する。このため、鋼板の材料は容易に塑性流動し、接合しようとする材料に高強度鋼板を用いても、容易にリベットを打ち込むことができる。
At that time, after the tip 7c of the rivet comes into contact with the steel plate 2, an electric current flows between the punch 4 and the die 6a, so that a current flows through the tip of the rivet and the steel plate, and the rivet and the steel plate are energized and heated.
Since the rivet tip 7c is sharp, current and stress are concentrated on the rivet tip and the steel plate in contact with the rivet tip during energization, and the temperature of the steel plate rises sharply. Therefore, the material of the steel sheet easily plastically flows, and even if a high-strength steel sheet is used as the material to be joined, rivets can be easily driven.

さらにポンチ4でリベット7を加圧してリベット先端部を鋼板内に侵入させる。リベット7の頭部7aのつば部が鋼板表面に到達した状態で、リベットの穿孔は停止し、加熱した状態でリベット7とダイ6a間の鋼板が加圧される。また、つば部を介してダイ6aとの間の鋼板も加圧される(図2d参照)。
リベットとダイの間で通電しながら、リベットを打ち込む際に、ポンチを冷却してもよく、その場合は、リベットの軟化を抑制して、より安定してリベットの打ち込みを行うことができる。
Further, the rivet 7 is pressed by the punch 4 to allow the tip of the rivet to penetrate into the steel plate. When the brim of the head portion 7a of the rivet 7 reaches the surface of the steel plate, the drilling of the rivet is stopped, and the steel plate between the rivet 7 and the die 6a is pressurized in a heated state. Further, the steel plate between the die 6a and the die 6a is also pressurized via the brim (see FIG. 2d).
The punch may be cooled when driving the rivet while energizing between the rivet and the die. In that case, softening of the rivet can be suppressed and the rivet can be driven more stably.

リベット7の頭部7bのつば部が鋼板2の内表面に到達した以降は、リベット7に付加する加圧力、印加する電流量、通電時間などを調整することにより、ダイ側の鋼板とリベット間が固相接合される場合(図2e参照)とダイ側の鋼板とリベット間が溶融接合される場合(図2f参照)に分かれる。 After the brim of the head portion 7b of the rivet 7 reaches the inner surface of the steel plate 2, the pressure applied to the rivet 7, the amount of current applied, the energization time, etc. are adjusted to be between the steel plate on the die side and the rivet. Is solid-phase bonded (see FIG. 2e) and melt-bonded between the steel plate on the die side and the rivet (see FIG. 2f).

(i)ダイ側の鋼板とリベットの間が固相接合される場合
通電加熱した状態で、鋼板とリベット間が加圧され、また、つば部を通して鋼板間も加圧される。この際に、リベットと鋼板の境界部や鋼板間の合わせ面が溶融しないように、加圧力や電流値を調整しながら通電加熱を継続することにより、リベットと鋼板の間および鋼板どうしの間で金属元素の相互拡散が進行し、両者が固相接合される(図2e参照)。
(I) When the steel plate and the rivet on the die side are solid-phase bonded The pressure is applied between the steel plate and the rivet while the steel plate and the rivet are energized and heated, and the steel plate is also pressurized through the brim. At this time, by continuing energization heating while adjusting the pressing force and current value so that the boundary between the rivet and the steel plate and the mating surface between the steel plates do not melt, between the rivet and the steel plate and between the steel plates. Mutual diffusion of metal elements progresses, and both are solid-phase bonded (see FIG. 2e).

(ii)ダイ側の鋼板とリベットの間が溶融接合される場合
リベットと鋼板間の通電電流を高める、加圧力を高めるなどにより、リベットの先端部と、該先端部に接している鋼板部分がともに溶融して、ナゲットが形成される。これにより、リベット鋼板間および鋼板間が、ナゲット9により溶融接合される(図2f参照)。
この場合は、図4に示すようにダイ6aのリベット7に対向する部分の面積を小さくして、鋼板の狭い領域に電流が集中して流れるようにすることが好ましい。
なお、鋼板が3枚以上の場合は、リベットの先端が最もダイ側の鋼板の内表面まで達するまでリベットを打ち込むのが好ましい。また、ダイ鋼板間の接合がより確実に行われる溶融接合の方が好ましい。
(Ii) When the steel plate on the die side and the rivet are melt-bonded The tip of the rivet and the steel plate in contact with the tip are brought into contact with each other by increasing the energizing current between the rivet and the steel plate or increasing the pressing force. Both melt to form a nugget. As a result, the rivet steel plates and the steel plates are melt-bonded by the nugget 9 (see FIG. 2f).
In this case, as shown in FIG. 4, it is preferable to reduce the area of the portion of the die 6a facing the rivet 7 so that the current is concentrated and flows in a narrow region of the steel sheet.
When there are three or more steel plates, it is preferable to drive the rivets until the tip of the rivet reaches the inner surface of the steel plate on the die side. Further, melt joining in which the joining between the die steel sheets is performed more reliably is preferable.

以上の結果、重ね合わされた鋼板は、リベットによる機械的接合と熱を利用した固相接合あるいは溶融接合の両方によって接合され、高強度鋼板を用いて剥離強度が十分に高い継手を形成することができる。 As a result of the above, the laminated steel sheets are joined by both mechanical joining by rivets and solid-state joining or melt joining using heat, and a high-strength steel sheet can be used to form a joint having sufficiently high peel strength. it can.

以上の実施形態では、ポンチ4とダイ6a間に通電する場合について説明したが、さらに、板押え5も電源装置に接続し、板押え5とダイ6a間に通電して、鋼板2、3を予備的に加熱することができる。
この場合、図2aのように鋼板をダイセット6と板押え5で挟んだ状態で、板押え5とダイ6a間に通電して、リベット先端7cが鋼板2に接触する前から鋼板を予備的に通電加熱する。次いで、ポンチ4を板押え5を通して鋼板側に移動させ、リベットの先端7cが鋼板2に接触した後、ポンチ4とダイ6a間に通電することにより、リベット先端と鋼板に電流が流れ、リベットと鋼板が通電加熱され、以降は、前記と同様にして、鋼板を接合する。
In the above embodiment, the case where the punch 4 and the die 6a are energized has been described. Further, the plate retainer 5 is also connected to the power supply device, the plate retainer 5 and the die 6a are energized, and the steel plates 2 and 3 are connected. Can be preheated.
In this case, with the steel plate sandwiched between the die set 6 and the plate retainer 5 as shown in FIG. 2a, energization is applied between the plate retainer 5 and the die 6a to prepare the steel plate before the rivet tip 7c comes into contact with the steel plate 2. Energize and heat. Next, the punch 4 is moved to the steel plate side through the plate retainer 5, and after the tip 7c of the rivet comes into contact with the steel plate 2, an electric current is applied between the punch 4 and the die 6a, so that a current flows through the rivet tip and the steel plate to form the rivet. The steel sheet is energized and heated, and thereafter, the steel sheet is joined in the same manner as described above.

このような本発明は、図5に概略を示すような、2段押付けを行うことができる接合装置11によって実施することが効果的である。
図において、接合しようとする鋼板2、3を間にして上方には、駆動装置(図示せず)により上下動するシャンク12の下端に、ダイセット6に組み付けられたダイ6aが配置される。また、下方には、同様に駆動装置(図示せず)により上下動するストレートホルダ13に、ダイ6aに対向してポンチ4が固定され、ポンチ4の外側には板押え5が配置され、ストレートホルダ13に固定されたアダプタ14にガススプリング15を介して板押え5を支持させている。
It is effective to carry out such an invention by a joining device 11 capable of performing two-stage pressing as outlined in FIG.
In the figure, a die 6a assembled to the die set 6 is arranged at the lower end of a shank 12 which is moved up and down by a driving device (not shown) above the steel plates 2 and 3 to be joined. Further, below, the punch 4 is fixed to the straight holder 13 which is similarly moved up and down by a driving device (not shown) so as to face the die 6a, and the plate retainer 5 is arranged on the outside of the punch 4 to be straight. The plate retainer 5 is supported by the adapter 14 fixed to the holder 13 via the gas spring 15.

接合動作中、ポンチ4をダイ6aに向けて駆動すると、板押え5もアダプタ14を介してダイ6aに向けて移動し、先に鋼板に当接して、鋼板をダイセット6とともに加圧保持する。ポンチ4がさらに上方に移動してリベット7を打ち込むようになると、ガススプリング15が圧縮して板押え5の加圧力がさらに増大して、鋼板2、3の合わせ面を密着させるようになっている。このため、合わせ面により電流が集中するようになる。 When the punch 4 is driven toward the die 6a during the joining operation, the plate retainer 5 also moves toward the die 6a via the adapter 14, first abuts on the steel plate, and pressurizes and holds the steel plate together with the die set 6. .. When the punch 4 moves further upward to drive the rivet 7, the gas spring 15 compresses and the pressing force of the plate retainer 5 further increases, so that the mating surfaces of the steel plates 2 and 3 are brought into close contact with each other. There is. Therefore, the current is concentrated on the mating surface.

鋼板への通電は、リベット7が鋼板3と接触した時にポンチ4とダイ6a間が導通することによって行われる。そのため、ポンチ4とダイ6aはそれぞれ電源装置8(図1参照)に接続される。さらに、リベット7が鋼板3と接触する前の板押え5が鋼板3と接触した時に、鋼板を通して板押え5とダイ6aを通電させ、鋼板を予備的に加熱するために、板押え5も電源装置8に接続することもできる。この場合には、より早く鋼板温度を上げることができる。 The energization of the steel plate is performed by the conduction between the punch 4 and the die 6a when the rivet 7 comes into contact with the steel plate 3. Therefore, the punch 4 and the die 6a are connected to the power supply device 8 (see FIG. 1), respectively. Further, when the plate retainer 5 before the rivet 7 contacts the steel plate 3 comes into contact with the steel plate 3, the plate retainer 5 and the die 6a are energized through the steel plate, and the plate retainer 5 is also supplied with power to preheat the steel plate. It can also be connected to the device 8. In this case, the temperature of the steel sheet can be raised faster.

ポンチ4がリベット7を打ち込む際、リベット7に後述するような所定のパターンの加圧力が負荷されるようにポンチ4の移動を制御する駆動制御手段が駆動装置に設けられている。また、電源装置8には、リベット7が鋼板と接触した時にポンチ4とダイ6a間が通電され、ポンチ4がリベット7を打ち込んでいる間、ポンチ4とダイ6a間に後述するような所定のパターンの電流が流れるように制御する通電制御手段が設けられている。さらに、板押え5とダイ6aが電源装置に接続されている場合は、通電制御手段は、板押え5が鋼板と接触した時に、鋼板を通して板押え5とダイ6aを通電させ、鋼板を予備的に加熱するように電流を制御する。 When the punch 4 drives the rivet 7, the drive device is provided with a drive control means for controlling the movement of the punch 4 so that the rivet 7 is loaded with a pressing force having a predetermined pattern as described later. Further, the power supply device 8 is energized between the punch 4 and the die 6a when the rivet 7 comes into contact with the steel plate, and while the punch 4 is driving the rivet 7, a predetermined value as described later is provided between the punch 4 and the die 6a. An energization control means for controlling the flow of the pattern current is provided. Further, when the plate retainer 5 and the die 6a are connected to the power supply device, the energization control means energizes the plate retainer 5 and the die 6a through the steel plate when the plate retainer 5 comes into contact with the steel plate to prepare the steel plate. Control the current to heat up.

以上、本発明の基本的な態様について説明したが、さらに本発明の個々の要件や好ましい要件についてさらに説明する。 The basic aspects of the present invention have been described above, and the individual requirements and preferable requirements of the present invention will be further described.

(接合対象とする鋼板)
鋼板は、上記例では2枚の鋼板で形成しているが、接合する構造部品の形態に応じて、3枚以上の複数の鋼板とすることができる。このような鋼板は、少なくとも一部に板状部を有し、当該板状部が互いに積み重ねられる部分を有するものであればよく、全体が板でなくともよい。また、別々の鋼板から構成されるものに限定されず、1枚の鋼板を管状に曲げ成形したものの端部を重ね合わせたものでよい。
(Steel sheet to be joined)
The steel plate is formed of two steel plates in the above example, but may be three or more steel plates depending on the form of the structural parts to be joined. Such a steel plate may have at least a plate-shaped portion at least in part and may have a portion in which the plate-shaped portions are stacked on each other, and the entire steel plate does not have to be a plate. Further, the method is not limited to the one composed of separate steel plates, and the end portions of one steel plate bent and formed into a tubular shape may be overlapped.

複数の鋼板には、780MPa級以上の鋼板を少なくとも1枚以上含むものとする。特に、全ての鋼板に780MPa級以上の鋼板を用いることにより、継手強度の高い部材を製造できることから、薄い鋼板の使用ができるようになり、部品の軽量化を達成できる。 The plurality of steel plates shall include at least one steel plate of 780 MPa class or higher. In particular, by using steel plates of 780 MPa class or higher for all steel plates, members having high joint strength can be manufactured, so that thin steel plates can be used, and weight reduction of parts can be achieved.

(リベット)
リベットは、一般的なリベットと同様に軸部とつば部を有する頭部よりなるもので、中実であり、軸部の先端部は釘状に尖っている。先端は、鋼板と接触して通電した時にすぐ加熱されて軟化するので、予め丸みを帯びていてもよい。
(rivet)
The rivet is composed of a head having a shaft portion and a brim portion like a general rivet, and is solid, and the tip portion of the shaft portion is pointed like a nail. The tip may be pre-rounded because it is immediately heated and softened when it comes into contact with the steel sheet and is energized.

リベットの材質は、鋼であれば特に限定されるものではないが、炭素量の低い鋼を用いることが好ましい。炭素量の低い鋼からなるリベットを用いることにより、接合部の硬さを抑制できるため、接合部のじん性が優れ、引張せん断強さや十字引張強さなどの継手強度を向上できる。また、ナゲットを形成する場合には、炭素量の低いナゲット部分を形成することができる。また接合部の硬さが低くなるため、高強度鋼板のスポット溶接部では発生が懸念される遅れ破壊(水素脆化)を抑制することも可能となる。この目的からは、特にC:0.15%以下の鋼が好ましい。 The material of the rivet is not particularly limited as long as it is steel, but it is preferable to use steel having a low carbon content. By using a rivet made of steel having a low carbon content, the hardness of the joint can be suppressed, so that the toughness of the joint is excellent and the joint strength such as tensile shear strength and cross tensile strength can be improved. Further, when forming a nugget, a nugget portion having a low carbon content can be formed. Further, since the hardness of the joint portion is lowered, it is possible to suppress delayed fracture (hydrogen embrittlement) which may occur in the spot welded portion of the high-strength steel plate. For this purpose, steel having a C: 0.15% or less is particularly preferable.

(ダイセット)
ダイセットは、ポンチや板押えと対向して配置され、板押えとの間でリベットの打ち込み中に鋼板を保持する押え部と、リベットの打ち込みに対し、鋼板の打ち込み面とは反対側の面が変形しないように鋼板を支えるダイよりなる。また、ダイは、リベットを通して鋼板を通電加熱する際の電極の作用もする。
押え部の材質は工具鋼とすればよいが、ダイは銅又は銅合金とすることが望ましい。
(Die set)
The die set is arranged so as to face the punch and the plate retainer, and holds the steel plate between the punch and the plate retainer during the driving of the rivet, and the surface opposite to the driving surface of the steel plate with respect to the driving of the rivet. Consists of a die that supports the steel plate so that it does not deform. The die also acts as an electrode when the steel sheet is energized and heated through the rivet.
The material of the presser foot may be tool steel, but the die is preferably copper or a copper alloy.

(ポンチ)
このポンチ4は、全体を通常の工具鋼で構成することもできるが、リベットに通電するための電極の作用もするため、リベットと接触する端部は電気伝導率が高い銅又は銅合金とすることが好ましい。
また、リベットを打ち込むとき、通電によりリベットの温度が上がりすぎる場合には、ポンチを冷却できるように、内部に冷却管を通して冷却するか、外から冷却する。
(Punch)
The punch 4 may be entirely made of ordinary tool steel, but since it also acts as an electrode for energizing the rivet, the end portion in contact with the rivet is made of copper or a copper alloy having high electrical conductivity. Is preferable.
When driving the rivet, if the temperature of the rivet rises too much due to energization, the punch is cooled by passing it through a cooling pipe inside or from the outside so that the punch can be cooled.

(板押え)
図5の例では、ガススプリングによって板押えを支持する例を示したが、ガススプリングに替えて、エアシリンダー、圧縮コイルバネ、適度な弾性を有するウレタン樹脂からなる樹脂成形体とすることもできる。
(Plate presser)
In the example of FIG. 5, an example in which the plate retainer is supported by a gas spring is shown, but instead of the gas spring, a resin molded body made of an air cylinder, a compression coil spring, and a urethane resin having appropriate elasticity can be used.

(加圧力と通電の条件)
リベットを鋼板に打ち込む際のポンチによる加圧力と鋼板を通電加熱するための電流のパターンとしては、(a)通常のスポット溶接のように、加圧力一定、電流(その実効値)一定とするパターン(図6a参照)や、(b)リベット先端と鋼板の温度が上昇したら、より高い加圧力と電流に増加させる2段階に変化させるパターンが例示できる。
(b)の場合は、ダイ側の鋼板とリベット間を溶融接合する場合に適しており、接合時間を短縮することができる。
(Conditions for pressurization and energization)
The patterns of the pressing force by the punch when driving the rivet into the steel plate and the current for energizing and heating the steel plate are as follows: (a) A pattern in which the pressing force is constant and the current (its effective value) is constant as in normal spot welding. (See FIG. 6a) and (b), when the temperature of the rivet tip and the steel plate rises, a pattern of changing to a higher pressing force and a current in two steps can be exemplified.
The case (b) is suitable for hot-dip joining between the steel plate on the die side and the rivet, and the joining time can be shortened.

電流と加圧力を2段階で変化させる場合は、電流を変化(増加)させるタイミングは加圧力を上昇させるタイミングとおよそ同時とするのがよい。1段目の第一電流で一定とする時間を第一通電時間とし、2段目の第二電流で一定とする時間を第二通電時間とすると、1段目の加圧力(第一加圧力)を保持する時間は、スポット溶接と同様に加圧力の安定を考慮して、第一通電時間より若干長めとする。具体的には、[第一加圧力の保持時間=スクイーズ時間+第一通電時間]とすればよい。ここでスクイーズ時間とは、加圧力の上昇時点から通電開始までの時間のことである。
また、2段目の第二加圧力を保持する時間は、接合を確実とするために、第二通電時間より若干長めとする。具体的には、[第二加圧力の保持時間=第二通電時間+保持時間]とすればよい。ここで保持時間とは、通電終了時点から加圧力保持を停止するまでの時間のことである。
When the current and the pressing force are changed in two steps, the timing of changing (increasing) the current should be approximately the same as the timing of increasing the pressing force. If the time that is constant at the first current of the first stage is the first energization time and the time that is constant at the second current of the second stage is the second energization time, the first stage pressurization (first pressurization) ) Is held for a little longer than the first energization time in consideration of the stability of the pressing force as in the case of spot welding. Specifically, it may be set as [holding time of first pressing force = squeeze time + first energizing time]. Here, the squeeze time is the time from the time when the pressing force rises to the start of energization.
Further, the time for holding the second pressing force in the second stage is set to be slightly longer than the second energizing time in order to ensure the joining. Specifically, it may be set as [holding time of second pressing force = second energizing time + holding time]. Here, the holding time is the time from the end of energization to the stop of holding the pressure.

以下実施例により本発明の実施可能性及び作用効果について説明する。
供試鋼として、板厚1.6mm、鋼板強度が1.8GPa級のS45C鋼からなる鋼板を2枚用い、この鋼板を重ねてスポット溶接または本発明のリベット接合を実施した。
The feasibility and action / effect of the present invention will be described below with reference to Examples.
As the test steel, two steel plates made of S45C steel having a plate thickness of 1.6 mm and a steel plate strength of 1.8 GPa class were used, and these steel plates were overlapped and spot welded or rivet-joined according to the present invention.

スポット溶接においては、加圧力、電流、通電時間を調整し、ナゲット径が約6mmとなるようにした。
一方、リベット接合においては、C量が0.12質量%の鋼製で、直径が6mm、首下(軸部)の長さが2.5mm、先端の開き角度が120°でつばの付いたリベットを用い、加圧力および電流を一定にする条件(図6a参照)か、または加圧力と電流値を2段階に変化させる条件(図6b参照)で接合を行った。
電流と加圧力を2段階で変化させる場合は、電流を変化(増加)させるタイミングを加圧力を上昇させるタイミングとおよそ同時とした。
全ての条件において、スクイーズ時間は0.5secとし、保持時間は0.2secとした。
それぞれの条件を表1に示す。
In spot welding, the pressing force, current, and energizing time were adjusted so that the nugget diameter was about 6 mm.
On the other hand, in the rivet joining, it is made of steel with a C content of 0.12% by mass, the diameter is 6 mm, the length under the neck (shaft) is 2.5 mm, the opening angle of the tip is 120 °, and the brim is attached. Using rivets, joining was performed under the condition that the pressing force and the current were constant (see FIG. 6a) or the pressing force and the current value were changed in two steps (see FIG. 6b).
When the current and the pressing force were changed in two steps, the timing of changing (increasing) the current was set to be approximately the same as the timing of increasing the pressing force.
Under all conditions, the squeeze time was 0.5 sec and the holding time was 0.2 sec.
Each condition is shown in Table 1.

得られた接合部の良否は継手強度(十字引張強さ=CTS)で判断した。
結果を表1に示すが、リベット接合のいずれの条件においても、そのCTSはスポット溶接継手のそれを上回った。リベット接合で2段通電を採用すると、1段通電の場合よりもCTSが向上しており、また接合に掛かる時間も短縮できていることが判る。
The quality of the obtained joint was judged by the joint strength (cross tensile strength = CTS).
The results are shown in Table 1, where the CTS outperformed that of spot welded joints under all conditions of riveting. It can be seen that when the two-stage energization is adopted for the rivet joining, the CTS is improved and the time required for the joining is shortened as compared with the case of the one-stage energization.

Figure 0006900692
Figure 0006900692

1 接合装置
2、3 接合しようとする重ね合わされた鋼板
4 ポンチ
5 板押え
6 ダイセット
6a ダイ
6b 押え部
7 リベット
7a リベットの軸部
7b リベットの頭部
7c 軸部の先端
8 電源装置
9 ナゲット
11 接合装置
12 シャンク
13 ストレートホルダ
14 アダプタ
15 ガススプリング
1 Joining device 2, 3 Overlapping steel plate to be joined 4 Punch 5 Plate presser 6 Die set 6a Die 6b Presser part 7 Rivet 7a Rivet shaft part 7b Rivet head 7c Shaft tip 8 Power supply device 9 Nugget 11 Joining device 12 Shank 13 Straight holder 14 Adapter 15 Gas spring

Claims (5)

引張強さが780MPa以上の高強度鋼板を少なくとも1枚は含む重ね合わせた複数枚の鋼板をセルフピアシングリベット、ポンチ及びダイを用いて接合する方法であって、
前記ポンチで、前記ポンチの外側にポンチと同軸に配置された板押えで鋼板を加圧しながら前記板押えと前記ダイ間に通電して、鋼板を予備的に加熱した後、
前記リベットとして、鋼よりなり先端部が尖った中実のリベットを用い、前記ポンチで前記リベットを加圧しながらリベットと前記ダイ間に通電して、前記接合しようとする鋼板を加熱しながら前記鋼板の厚み方向の所定の位置までリベットを押し込み、さらにポンチでリベットを加圧しながら通電を継続して、少なくとも鋼板間を固相接合あるいは溶融接合することを特徴とする接合方法。
A method of joining a plurality of stacked steel sheets including at least one high-strength steel sheet having a tensile strength of 780 MPa or more by using a self-piercing rivet, a punch and a die.
After the steel plate is preheated by energizing between the plate retainer and the die while pressurizing the steel plate with the punch, which is arranged coaxially with the punch on the outside of the punch.
As the rivet, said steel sheet using a solid rivet having a sharp tip made of steel, by energizing between the rivet and the die while pressing the rivet in the punch, while heating the steel sheet to be the joint A joining method characterized in that a rivet is pushed to a predetermined position in the thickness direction of the steel sheet, and then energization is continued while pressurizing the rivet with a punch to perform solid-phase bonding or melt-bonding at least between steel sheets.
前記リベットとして、C:0.15質量%以下の鋼を用いることを特徴とする請求項1に記載の接合方法。 The joining method according to claim 1, wherein a steel having a C content of 0.15% by mass or less is used as the rivet. 前記ポンチで前記リベットを加圧しながら前記リベットと前記ダイ間に通電する工程において、In the step of energizing between the rivet and the die while pressurizing the rivet with the punch.
第一電流及び第一加圧力で通電加圧した後、第一電流よりも高い第二電流、及び、第一加圧力よりも高い第二加圧力で通電加圧することを特徴とする請求項1又は2に記載の接合方法。 Claim 1 is characterized in that after energization and pressurization with a first current and a first pressurization, energization and pressurization is performed with a second current higher than the first current and a second pressurization higher than the first pressurization. Or the joining method according to 2.
請求項に記載の接合方法の実施に使用する接合装置であって、互いに対向する一方の側に、ポンチと該ポンチの外側にポンチと同軸に設けられた筒状の板押えを有し、他方の側に、接合しようとする鋼板をポンチに対向して支持するダイを有し、
前記板押えとダイ、前記ポンチとダイがそれぞれ電源装置に接続され、
前記板押えが鋼板と接触した時に板押えとダイ間が通電して鋼板を予備的に加熱した後、
前記リベットが鋼板と接触した時に前記ポンチとダイ間が通電して鋼板をさらに加熱するように構成されていることを特徴とする接合装置。
A joining device used to carry out the joining method according to claim 1 , which has a punch and a tubular plate retainer coaxially provided on the outside of the punch on one side facing each other. On the other side, it has a die that supports the steel plate to be joined against the punch.
The plate retainer and die, and the punch and die are connected to the power supply device, respectively.
When the plate retainer comes into contact with the steel plate, the plate retainer and the die are energized to preheat the steel plate, and then
A joining device characterized in that when the rivet comes into contact with a steel sheet, the punch and the die are energized to further heat the steel sheet.
請求項3に記載の接合方法の実施に使用する接合装置であって、A joining device used to carry out the joining method according to claim 3.
一方の側に、ポンチと、該ポンチの外側にポンチと同軸に設けられた筒状の板押えを有し、他方の側に、接合しようとする鋼板をポンチに対向して支持するダイを有し、One side has a punch and a tubular plate retainer coaxially provided on the outside of the punch, and the other side has a die that supports the steel plate to be joined facing the punch. And
前記板押えとダイ、前記ポンチとダイがそれぞれ電源装置に接続され、The plate retainer and die, and the punch and die are connected to the power supply device, respectively.
前記板押えが鋼板と接触した時に板押えとダイ間が通電して鋼板を予備的に加熱した後、When the plate retainer comes into contact with the steel plate, the plate retainer and the die are energized to preheat the steel plate, and then
前記リベットが鋼板と接触した時に前記ポンチとダイ間が通電して鋼板をさらに加熱するように構成され、かつ、When the rivet comes into contact with the steel sheet, the punch and the die are energized to further heat the steel sheet, and
前記ポンチとダイ間が通電して鋼板をさらに加熱する際に、第一電流及び第一加圧力で通電加圧した後、第一電流よりも高い第二電流、及び、第一加圧力よりも高い第二加圧力で通電加圧するように構成されていることを特徴とする接合装置。When the punch and the die are energized to further heat the steel sheet, after energizing and pressurizing with the first current and the first pressing force, the second current higher than the first current and the first pressing force A joining device characterized in that it is configured to be energized and pressurized with a high second pressing force.
JP2017020504A 2017-02-07 2017-02-07 Joining method using rivets and equipment used for its implementation Active JP6900692B2 (en)