JP5410026B2 - Sanitary tissue paper - Google Patents

Sanitary tissue paper Download PDF

Info

Publication number
JP5410026B2
JP5410026B2 JP2008068292A JP2008068292A JP5410026B2 JP 5410026 B2 JP5410026 B2 JP 5410026B2 JP 2008068292 A JP2008068292 A JP 2008068292A JP 2008068292 A JP2008068292 A JP 2008068292A JP 5410026 B2 JP5410026 B2 JP 5410026B2
Authority
JP
Japan
Prior art keywords
paper
softener
carbon atoms
component
softening agent
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
JP2008068292A
Other languages
Japanese (ja)
Other versions
JP2009221631A (en
Inventor
敦嗣 小沼
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Daio Paper Corp
Original Assignee
Daio Paper Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Daio Paper Corp filed Critical Daio Paper Corp
Priority to JP2008068292A priority Critical patent/JP5410026B2/en
Publication of JP2009221631A publication Critical patent/JP2009221631A/en
Application granted granted Critical
Publication of JP5410026B2 publication Critical patent/JP5410026B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Description

本発明は、柔軟性に加えて滑らかさを向上させた衛生用薄葉紙に関するものである。   The present invention relates to a sanitary thin paper having improved smoothness in addition to flexibility.

ティシュペーパー等の衛生用薄葉紙は、安価な使い捨て物品として様々な用途に利用されている。特に、鼻かみや口ふき等、フェイシャル用途に代表さる清拭用途に使用されることが多い。
そして、この種の衛生用薄葉紙は、かかる用途に用いられるため、例えば、花粉症の時期等、頻繁に鼻をかむ際に皮脂が奪われて鼻を赤くしてしまうという問題や、口周りなどの皮膚の弱い部分を拭く際に摩擦によって皮膚を痛めるおそれがあるという問題を抱える。従って、この種の衛生用薄葉紙においては、摩擦による皮膚への影響を低減すべく、柔らかであることが重要とされており、その改善に努められてきた。
しかし、上記皮膚に対する問題点においては、柔軟性を高めるだけでは改善しきれず、滑らかな肌触りも重要なファクターであることが知見された。
そしてこのような滑らかさは、柔軟剤を基材紙に多量に含有させることで改善されるが、柔軟性を高めるべく柔軟剤を多量に用いると、余剰の柔軟剤の発泡等や余剰柔軟剤の凝集等によるカスの発生に起因する操業上のトラブルが生じたり、紙力の低下を招くおそれがあった。
特開2006−307403 特許3322735号
Sanitary thin paper such as tissue paper is used in various applications as an inexpensive disposable article. In particular, it is often used for wiping applications such as nose bites and mouth wipes, such as facial applications.
And since this type of sanitary thin paper is used for such applications, for example, the time of pollinosis, the problem that sebum is taken away frequently when biting the nose, the nose becomes red, etc. When wiping a weak part of the skin, there is a problem that it may hurt the skin by friction. Therefore, in this type of sanitary thin paper, it is important to be soft in order to reduce the influence on the skin due to friction, and efforts have been made to improve it.
However, it has been found that the above-mentioned problems with the skin cannot be improved only by increasing the flexibility, and that smooth touch is also an important factor.
Such smoothness can be improved by adding a large amount of a softening agent to the base paper. However, if a large amount of softening agent is used to increase flexibility, foaming of excess softening agent or surplus softening agent is used. There is a risk that operational troubles may occur due to the generation of debris due to flocculation or the like, and the paper strength may be reduced.
JP 2006-307403 A Japanese Patent No. 3322735

そこで、本発明の主たる課題は、柔らかさに加えて滑らかさ感がより向上され、しかも紙力の低下なく、生産上のトラブルも解消できる、衛生用薄葉紙を提供することにある。   Therefore, a main object of the present invention is to provide a sanitary thin paper that has a feeling of smoothness in addition to softness, and that can solve problems in production without lowering paper strength.

上記課題を解決した本発明は次記のとおりである。
<請求項1記載の発明>
基材紙に対して薄葉紙処理剤を含有させた衛生用薄葉紙であって、
前記薄葉紙処理剤が柔軟剤と柔軟剤定着補助剤とを含み、
前記柔軟剤が、
アルキル基及び/又はアルケニル基を有する非イオン性界面活性剤(A成分)とアルキル基及び/又はアルケニル基を有するカチオン性界面活性剤(B成分)とを含有し、それらの固形分重量比がA成分/B成分=100/0.5〜100/20であり、
前記A成分が下記一般式(1)、(2)及び(3)で表される化合物の少なくとも一種であり、
1−A1−(EO)m(PO)n−CO−R2 ・・・(1)
1−O−(EO)m(PO)n−R2 ・・・(2)
1−A1−(EO)m(PO)nH ・・・(3)
(但し、式中、−A1−は−O−又は−COO−を示し、R1とR2とは炭素数6〜24のアルキル基又は炭素数6〜24のアルケニル基を示し、かつR1とR2とは同一又は相異してもよく、Eはエチレン基を示し、Pはプロピレン基を示し、mとnとの合計は1〜60である。なお、m及びnは平均付加モル数である。)
前記B成分がアルキル基及び/又はアルケニル基を有するイミダゾリン環を有する4級アンモニウム塩、又は下記一般式(4)で表される化合物であり、

Figure 0005410026
前記柔軟剤定着補助剤が、
ポリアミド・エピクロロヒドリン樹脂であり、
前記柔軟剤と柔軟剤定着補助剤の質量比が2.8:2.5〜10:1であり、
かつ、柔軟剤の含有量が0.7〜2.8kg/tであり、柔軟剤定着補助剤の含有量が0.1〜2.5kg/tであり、
JIS P 8113に規定される乾燥引張強度が、縦方向200〜350cN/25mm、横方向90〜140cN/25mmであり、かつ、
澱粉、カチオン性澱粉、カチオン性変成澱粉、カルボキシメチルセルロース若しくはその塩であるカルボキシメチルセルロースナトリウム、カルボキシメチルセルロースカルシウム、カルボキシメチルセルロース亜鉛が含有されていない、
ことを特徴とする衛生用薄葉紙。 The present invention that has solved the above problems is as follows.
<Invention of Claim 1>
A sanitary thin paper containing a thin paper treating agent for a base paper,
The tissue paper treating agent includes a softening agent and a softening agent fixing aid,
The softener is
A nonionic surfactant having an alkyl group and / or alkenyl group (component A) and a cationic surfactant having an alkyl group and / or alkenyl group (component B), and the solid content weight ratio thereof is A component / B component = 100 / 0.5 to 100/20,
The component A is at least one compound represented by the following general formulas (1), (2) and (3),
R 1 -A 1- (EO) m (PO) n -CO-R 2 (1)
R 1 —O— (EO) m (PO) n —R 2 (2)
R 1 -A 1- (EO) m (PO) n H (3)
(In the formula, —A 1 — represents —O— or —COO—, R 1 and R 2 represent an alkyl group having 6 to 24 carbon atoms or an alkenyl group having 6 to 24 carbon atoms, and R 1 and R 2 may be the same or different, E represents an ethylene group, P represents a propylene group, and the sum of m and n is 1 to 60, where m and n are average additions Number of moles.)
The B component is a quaternary ammonium salt having an imidazoline ring having an alkyl group and / or an alkenyl group, or a compound represented by the following general formula (4):
Figure 0005410026
The softener fixing auxiliary agent is
A polyamide / epichlorohydrin resin,
The mass ratio of the softener and softener fixing aid is 2.8: 2.5-10: 1;
And content of a softening agent is 0.7-2 . 8 kg / t, the content of the softener fixing auxiliary is 0.1 to 2.5 kg / t,
The dry tensile strength defined in JIS P 8113 is 200 to 350 cN / 25 mm in the longitudinal direction, 90 to 140 cN / 25 mm in the transverse direction, and
Contains no starch, cationic starch, cationic modified starch, carboxymethylcellulose or its salt, carboxymethylcellulose sodium, carboxymethylcellulose calcium, carboxymethylcellulose zinc,
Hygienic thin paper characterized by that.

以上の本発明によれば、トラブルなく製造可能であり、しかも柔らかさに加えて、滑らかさがより向上された薄葉紙が提供される。   According to the present invention described above, a thin paper that can be produced without any trouble and that has improved smoothness in addition to softness is provided.

以下、本発明の実施形態について詳説する。
本発明の衛生用薄葉紙は、基材紙に対して薄葉紙処理剤が含有されているものである。
〔基材紙〕
前記基材紙は、そのプライ数は限定されず、衛生用薄葉紙の用途等に応じて適宜選択することができる。
ただし、1プライ当たりの米坪(JIS P 8124)は10.0〜25.0g/m2が望ましい。米坪が10.0g/m2よりも小さいと、十分な強度を保つことができず製造時に破れ、断紙等の原因となる。また米坪が25.0g/m2よりも大きいと紙力を下げる事ができなくなるだけでなく、柔軟剤を添加した際の効果が分かりにくくなる。
Hereinafter, embodiments of the present invention will be described in detail.
The sanitary thin paper of the present invention contains a thin paper treating agent relative to the base paper.
[Base paper]
The number of plies of the base paper is not limited and can be appropriately selected according to the use of sanitary thin paper.
However, it is desirable that the rice tsubo per ply (JIS P 8124) is 10.0 to 25.0 g / m 2 . When the rice tsubo is smaller than 10.0 g / m 2 , sufficient strength cannot be maintained, and it is torn at the time of manufacture, causing paper breakage or the like. On the other hand, if the rice tsubo is larger than 25.0 g / m 2 , not only the paper strength cannot be lowered, but also the effect when the softening agent is added becomes difficult to understand.

他方、本発明の衛生用薄葉紙の基材紙は、上記坪量の範囲において、既知の抄紙原料を既知の抄紙技術によって抄造したものを用いることができるが、特に抄紙原料中のパルプ原料おけるNBKP配合率(JIS P 8120)が30.0〜80.0%、特に40.0〜70.0%であるものが好適である。   On the other hand, the base paper of the sanitary thin paper of the present invention can be obtained by making a known papermaking raw material by a known papermaking technique within the range of the basis weight. A blending ratio (JIS P 8120) of 30.0 to 80.0%, particularly 40.0 to 70.0% is preferred.

また、原紙の紙力調整は米坪以外にも抄紙用澱粉やフリーネスの調整によっても行うことができる。原料パルプ未叩解時のフリーネス(ろ水度)はJIS P 8121に準じたカナダ標準ろ水度試験法から500〜700CC程度である。これを未叩解又は叩解することでフリーネスダウン幅を0〜50CC程度とすることで、柔軟剤、滑らかさを維持すると共に、原紙の強度をもたせることができる。   Further, the paper strength of the base paper can be adjusted by adjusting the starch for papermaking and the freeness in addition to the rice tsubo. The freeness (freeness) when raw pulp is not beaten is about 500 to 700 CC based on the Canadian standard freeness test method according to JIS P8121. By setting the freeness down width to about 0 to 50 CC by unbeating or beating this, the softening agent and smoothness can be maintained and the strength of the base paper can be given.

〔薄葉紙処理剤〕
他方、前記薄葉紙処理剤は、柔軟剤と柔軟剤定着補助剤を含む。
(柔軟剤)
本発明にかかる柔軟剤は、アルキル基及び/ 又はアルケニル基を有する非イオン性界面活性剤(A 成分)とアルキル基及び/ 又はアルケニル基を有するカチオン性界面活性剤(B成分) とを含有する。
[Thin paper treatment agent]
On the other hand, the thin paper treating agent includes a softening agent and a softening agent fixing auxiliary agent.
(Softener)
The softener according to the present invention contains a nonionic surfactant having an alkyl group and / or alkenyl group (component A) and a cationic surfactant having an alkyl group and / or alkenyl group (component B). .

まず、前記非イオン性界面活性剤(A成分)について説明する。この非イオン性界面活性剤(A成分)は、アルキル基及び/ 又はアルケニル基を有し、炭素数6〜24のアルキル基及び/ 又は炭素数6〜24のアルケニル基を疎水部として有することが好ましい。   First, the nonionic surfactant (component A) will be described. This nonionic surfactant (component A) has an alkyl group and / or alkenyl group, and has an alkyl group having 6 to 24 carbon atoms and / or an alkenyl group having 6 to 24 carbon atoms as a hydrophobic portion. preferable.

本発明において、A成分の炭素数が6未満であると柔軟効果が高まらない場合があり、炭素数が24を超えると抄紙系に添加した際の分散性が悪くなったりする場合がある。従って、本発明にかかるA成分の炭素数は6〜24の範囲であることが好ましい。   In the present invention, if the carbon number of the component A is less than 6, the flexibility effect may not be enhanced, and if the carbon number exceeds 24, the dispersibility when added to the papermaking system may deteriorate. Therefore, the carbon number of the component A according to the present invention is preferably in the range of 6-24.

このような非イオン性界面活性剤としては、高級アルコール又は高級脂肪酸にオキシアルキレン基が付加した非イオン性界面活性剤、多価アルコールと脂肪酸とのエステル、および下記一般式(1)および(2)で表される化合物( 以下化合物Iとする) を挙げることができる。これらは単独で用いても良いし、二種以上を併用しても良い。   As such a nonionic surfactant, a nonionic surfactant in which an oxyalkylene group is added to a higher alcohol or higher fatty acid, an ester of a polyhydric alcohol and a fatty acid, and the following general formulas (1) and (2) ) (Hereinafter referred to as Compound I). These may be used alone or in combination of two or more.

高級アルコール又は高級脂肪酸にオキシアルキレン基が付加した非イオン性界面活性剤としては、下記一般式(3)で表される化合物を挙げることができる。
R1−A1−(EO)m(PO )n−CO−R2 ・・・( 1 )
R1−O−(EO m(PO)n−R2 ・・・( 2 )
R1−A1−(EO)m(PO)nH ・・・( 3 )
( 但し、式中、−A1−は−O−又は−COO−を示し、R1とR2とは炭素数6〜24、好ましくは10〜22のアルキル基又は炭素数6〜24、好ましくは10〜22のアルケニル基を示し、かつR1とR2とは同一又は相異していてもよく、E はエチレン基を示し、Pはプロピレン基を示し、mとnとの合計は1〜60、好ましくは2〜40である。なお、m及びnは平均付加モル数である。)
Examples of the nonionic surfactant in which an oxyalkylene group is added to a higher alcohol or a higher fatty acid include compounds represented by the following general formula (3).
R1-A1- (EO) m (PO) n-CO-R2 (1)
R1-O- (EO m (PO) n-R2 (2)
R1-A1- (EO) m (PO) nH (3)
(However, in the formula, -A1- represents -O- or -COO-, and R1 and R2 represent an alkyl group having 6 to 24 carbon atoms, preferably 10 to 22 carbon atoms, or 6 to 24 carbon atoms, preferably 10 to 10 carbon atoms. 22 represents an alkenyl group, and R1 and R2 may be the same or different, E represents an ethylene group, P represents a propylene group, and the sum of m and n is 1 to 60, preferably 2 to 40, where m and n are the average number of moles added.)

一般式(1)〜(3)で示される非イオン性界面活性剤のうち、一般式(1)及び(2) で示される非イオン性界面活性剤が好ましく、更に好ましくは一般式(1)で示される非イオン性界面活性剤である。    Of the nonionic surfactants represented by the general formulas (1) to (3), the nonionic surfactants represented by the general formulas (1) and (2) are preferable, and the general formula (1) is more preferable. It is a nonionic surfactant shown by these.

上記一般式(1)で表される化合物は、例えば炭素数が6〜24、好ましくは10〜22のアルコール又は炭素数が7〜27、好ましくは11〜23の脂肪酸1モルにエチレンオキサイド、及び/ 又はプロピレンオキサイドを付加した後に、炭素数が7〜25、好ましくは11〜23の脂肪酸1モルでエステル化して得ることができる。エチレンオキサイド、及び/ 又はプロピレンオキサイドの付加形態はランダムでもブロックでも良く、炭素数が6〜24、好ましくは10〜22のアルコール又は炭素数7〜25、好ましくは11 〜23の脂肪酸1モルに対して1〜60モル、好ましくは2〜40モルの割合で付加される。60モルを超えると、柔軟効果が低くなることがある。   The compound represented by the general formula (1) is, for example, an alcohol having 6 to 24 carbon atoms, preferably 10 to 22 alcohols or 7 to 27 carbon atoms, preferably 1 to 23 moles of fatty acids having 11 to 23 carbon atoms, and After addition of propylene oxide, it can be obtained by esterification with 1 mol of a fatty acid having 7 to 25 carbon atoms, preferably 11 to 23 carbon atoms. The addition form of ethylene oxide and / or propylene oxide may be random or block, and is an alcohol having 6 to 24 carbon atoms, preferably 10 to 22 carbon atoms or 1 mol of fatty acid having 7 to 25 carbon atoms, preferably 11 to 23 carbon atoms. 1 to 60 mol, preferably 2 to 40 mol. When it exceeds 60 mol, the softening effect may be lowered.

上記一般式(2)で表される化合物は、例えば炭素数が6〜24 、好ましくは10〜22のアルコール1モルにエチレンオキサイド、及び/ 又はプロピレンオキサイドを付加したのちに、炭素数が6〜24、好ましくは10〜22のアルコールまたは炭素数が6〜24、好ましくは1 0 〜 2 2 のハロゲン化アルキル1 モルでエーテル化して得ることができる。エチレンオキサイド、及び/ 又はプロピレンオキサイドの付加形態はランダムでもブロックでも良く、炭素数が6〜24、好ましくは10〜22のアルコール1モルに対して1〜60モル、好ましくは2〜40モルの割合で付加される。60モルを超えると、柔軟効果が低下させることがある。   The compound represented by the general formula (2) has, for example, 6 to 24 carbon atoms, preferably 6 to 22 carbon atoms after adding ethylene oxide and / or propylene oxide to 1 mole of alcohol having 10 to 22 carbon atoms. It can be obtained by etherification with 24, preferably 10 to 22 alcohols or 1 mole of alkyl halide with 6 to 24, preferably 10 to 22 carbon atoms. The addition form of ethylene oxide and / or propylene oxide may be random or block, and a ratio of 1 to 60 mol, preferably 2 to 40 mol, per 1 mol of alcohol having 6 to 24 carbon atoms, preferably 10 to 22 carbon atoms. It is added with. When it exceeds 60 mol, the softening effect may be lowered.

上記一般式(3)で表される化合物は、例えば炭素数が6〜24、好ましくは10〜22のアルコール又は炭素数が7〜25、好ましくは11〜23の脂肪酸1モルにエチレンオキサイド、及び/ 又はプロピレンオキサイドを付加して得ることができる。エチレンオキサイド、及び/ 又はプロピレンオキサイドの付加形態はランダムでもブロックでも良く、炭素数が6〜24、好ましくは10〜22のアルコール又は炭素数7〜25、好ましくは11〜23の脂肪酸1モルに対して1〜60モル、好ましくは2〜40の割合で付加される。60モルを超えると、柔軟効果が低下させることがある。   The compound represented by the general formula (3) is, for example, an alcohol having 6 to 24 carbon atoms, preferably 10 to 22 alcohols or 7 to 25 carbon atoms, preferably 1 to 23 moles of fatty acids having 11 to 23 carbon atoms, and / Or it can be obtained by adding propylene oxide. The addition form of ethylene oxide and / or propylene oxide may be random or block, and is an alcohol having 6 to 24 carbon atoms, preferably 10 to 22 carbon atoms, or 1 mol of fatty acid having 7 to 25 carbon atoms, preferably 11 to 23 carbon atoms. 1 to 60 mol, preferably 2 to 40 mol. When it exceeds 60 mol, the softening effect may be lowered.

炭素数が6〜24のアルコールとしては、直鎖アルコール、分岐鎖を有するアルコール、飽和アルコール、及び不飽和アルコールの何れでも良い。これら各種のアルコールの中でも炭素数が10〜22のアルコールが好ましく、特に、ラウリルアルコール、ミリスチルアルコール、セチルアルコール、ステアリルアルコール、ベヘニルアルコール、及びオレイルアルコールが好ましい。これらはその一種を単独で用いても良いし、二種以上を併用しても良い。   The alcohol having 6 to 24 carbon atoms may be any of linear alcohol, branched chain alcohol, saturated alcohol, and unsaturated alcohol. Among these various alcohols, alcohols having 10 to 22 carbon atoms are preferable, and lauryl alcohol, myristyl alcohol, cetyl alcohol, stearyl alcohol, behenyl alcohol, and oleyl alcohol are particularly preferable. These may be used alone or in combination of two or more.

炭素数7〜25の脂肪酸としては、直鎖脂肪酸、分岐鎖を有する脂肪酸、飽和脂肪酸、及び不飽和脂肪酸の何れでも良い。これら各種の脂肪酸の中でも、炭素数が10〜22の脂肪酸が好ましく、特に、ラウリン酸、ミリスチン酸、パルミチン酸、ステアリン酸、ベヘン酸、及びオレイン酸が好ましい。これらはその一種を単独で用いても良いし、二種以上を併用しても良い。   The fatty acid having 7 to 25 carbon atoms may be any of linear fatty acid, fatty acid having a branched chain, saturated fatty acid, and unsaturated fatty acid. Among these various fatty acids, fatty acids having 10 to 22 carbon atoms are preferable, and lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, and oleic acid are particularly preferable. These may be used alone or in combination of two or more.

他方、前記カチオン性界面活性剤(B成分)としては、第1級アミン類、第2級アミン類、第3級アミン類、及び第4級アンモニウム塩などが挙げられる。これらはその一種を単独で用いても良いし、二種以上を併用しても良い。特に、第4級アンモニウム塩が好ましい。   On the other hand, examples of the cationic surfactant (component B) include primary amines, secondary amines, tertiary amines, and quaternary ammonium salts. These may be used alone or in combination of two or more. In particular, a quaternary ammonium salt is preferable.

第1級アミン類としては下記一般式で表される化合物
R8−NH2 ・・・( 6 )
( 但し、式中、R8は、炭素数6〜24のアルキル基、炭素数6〜24のアルケニル基から選ばれる1 種を示す。)具体例としてはオレイルアミン、ラウリルアミン、ステアリルアミンが挙げられる。
As primary amines, compounds represented by the following general formula: R8-NH2 (6)
(In the formula, R8 represents one selected from an alkyl group having 6 to 24 carbon atoms and an alkenyl group having 6 to 24 carbon atoms.) Specific examples include oleylamine, laurylamine, and stearylamine.

第2級アミン類としては下記一般式で表される化合物
R9R10−NH ・・・( 7 )
( 但し、式中、R9は、炭素数6〜24のアルキル基、炭素数6〜24のアルケニル基から選ばれる1種を示し、R10は(EO)m(PO)nH、炭素数1〜24のアルキル基、炭素数1〜24のアルケニル基から選ばれる1種を示し、前記Eはエチレン基を示し、前記Pはプロピレン基を示し、mとnとの合計は1〜60である。なお、m及びnは平均付加モル数である。)
具体例としてはジオレイルアミン、モノオレイルモノメチルアミンが挙げられる。
Secondary amines are compounds represented by the following general formula: R9R10-NH (7)
(In the formula, R9 represents one selected from an alkyl group having 6 to 24 carbon atoms and an alkenyl group having 6 to 24 carbon atoms, and R10 is (EO) m (PO) nH, 1 to 24 carbon atoms). 1 is selected from an alkyl group having 1 to 24 carbon atoms, E is an ethylene group, P is a propylene group, and the sum of m and n is 1 to 60. , M and n are the average number of moles added.)
Specific examples include dioleylamine and monooleyl monomethylamine.

第3級アミン類としては下記一般式で表される化合物
R11R12R13N ・・・( 8 )
( 但し、式中、R11は、炭素数6〜24のアルキル基、炭素数6〜24のアルケニル基から選ばれる1種を示し、R12とR13とは(EO)m(PO)nH、炭素数1〜24のアルキル基、及び炭素数1〜24のアルケニル基から選ばれる1種を示し、かつR12とR13とは同一であっても相違していてもよく、前記E はエチレン基を示し、前記P はプロピレン基を示し、mとnとの合計は1〜60である。なお、m及びnは平均付加モル数である。)
この第3 級アミン類の具体例としてはポリオキシアルキレンジオレイルアミン、ポリオキシアルキレンエチレングリコールラウリルアミン、ジメチルモノオレイルアミン、モノメチルジオレイルアミンが挙げられる。
Tertiary amines are compounds represented by the following general formula: R11R12R13N (8)
(In the formula, R11 represents one selected from an alkyl group having 6 to 24 carbon atoms and an alkenyl group having 6 to 24 carbon atoms, and R12 and R13 are (EO) m (PO) nH, carbon number) 1 type | mold chosen from a C1-C24 alkyl group and a C1-C24 alkenyl group, and R12 and R13 may be the same or different, Said E shows an ethylene group, P 1 represents a propylene group, and the sum of m and n is 1 to 60, where m and n are the average number of moles added.
Specific examples of the tertiary amines include polyoxyalkylene dioleyl amine, polyoxyalkylene ethylene glycol lauryl amine, dimethyl monooleyl amine, and monomethyl dioleyl amine.

第4級アンモニウム塩としては、下記一般式(4)で表される化合物、及び下記一般式(5)のイミダゾリン環を有する4 級塩などが挙げられる。これらはその一種を単独で用いても良いし、二種以上を併用しても良い。

Figure 0005410026
( 但し、式中、R3は炭素数6〜24のアルキル基又は炭素数6〜24のアルケニル基を、R4とR5とは(EO)m(PO)nH、炭素数1〜24のアルキル基、及び炭素数1〜24のアルケニル基から選ばれる1種を示し、かつR4とR5とは同一又は相異していてもよく、X−は陰イオンであり、前記Eはエチレン基を示し、前記Pはプロピレン基を示し、mとnとの合計は1〜60である。エチレンオキサイド、及び/ 又はプロピレンオキサイドの付加形態はランダムでもブロックでも良い。なお、m及びnは平均付加モル数である。)
上記一般式(4)で表される第4 級アンモニウム塩としては、具体的にはトリメチルモノラウリルアンモニウムクロライド、トリメチルモノセチルアンモニウムクロライド、トリメチルモノパルミチルアンモニウムクロライド、トリメチルモノステアリルアンモニウムクロライド、トリメチルモノオレイルアンモニウムクロライド、トリメチルモノベヘニルアンモニウムクロライド、ジメチルジラウリルアンモニウムクロライド、ジメチルジセチルアンモニウムクロライド、ジメチルジパルミチルアンモニウムクロライド、ジメチルジステアリルアンモニウムクロライド、ジメチルジオレイルアンモニウムクロライド、ジメチルジベヘニルアンモニウムクロライド、ポリアルキレンオキシモノメチルジオレイルアンモニウムクロライド、ビス( ポリアルキレンオキシ) モノメチルモノオレイルアンモニウムクロライドが挙げられる。
このなかでもトリメチルモノステアリルアンモニウムクロライド、トリメチルモノオレイルアンモニウムクロライド、ジメチルジラウリルアンモニウムクロライド、ジメチルジオレイルアンモニウムクロライド、ポリアルキレンオキシモノメチルジオレイルアンモニウムクロライド、ビス( ポリアルキレンオキシ) モノメチルモノオレイルアンモニウムクロライドが好ましい。 Examples of the quaternary ammonium salt include a compound represented by the following general formula (4) and a quaternary salt having an imidazoline ring represented by the following general formula (5). These may be used alone or in combination of two or more.
Figure 0005410026
(In the formula, R3 is an alkyl group having 6 to 24 carbon atoms or an alkenyl group having 6 to 24 carbon atoms, R4 and R5 are (EO) m (PO) nH, an alkyl group having 1 to 24 carbon atoms, And R4 and R5 may be the same or different from each other, X- is an anion, E represents an ethylene group, P represents a propylene group, and the total of m and n is 1 to 60. The addition form of ethylene oxide and / or propylene oxide may be random or block, where m and n are the average number of moles added. .)
Specific examples of the quaternary ammonium salt represented by the general formula (4) include trimethyl monolauryl ammonium chloride, trimethyl monocetyl ammonium chloride, trimethyl monopalmityl ammonium chloride, trimethyl monostearyl ammonium chloride, trimethyl monooleyl. Ammonium chloride, trimethyl monobehenyl ammonium chloride, dimethyl dilauryl ammonium chloride, dimethyl dicetyl ammonium chloride, dimethyl dipalmityl ammonium chloride, dimethyl distearyl ammonium chloride, dimethyl dioleyl ammonium chloride, dimethyl dibehenyl ammonium chloride, polyalkyleneoxy monomethyl Dioleyl ammonium chloride, bis (Polyalkyleneoxy) Monomethyl monooleyl ammonium chloride is exemplified.
Among these, trimethyl monostearyl ammonium chloride, trimethyl monooleyl ammonium chloride, dimethyl dilauryl ammonium chloride, dimethyl dioleyl ammonium chloride, polyalkyleneoxy monomethyl dioleyl ammonium chloride, and bis (polyalkyleneoxy) monomethyl monooleyl ammonium chloride are preferable.

イミダゾリン環を有する4級アンモニウム塩としては、下記一般式(5)で表される化合物を挙げることができる。これらを単独で用いても良いし、二種以上を併用しても良い。

Figure 0005410026
( 但し、式中、R6は炭素数6〜24のアルキル基又は炭素数6〜24のアルケニル基を、R7は炭素数1〜24のアルキル基又は炭素数1〜24のアルケニル基を示し、X− は陰イオンである。) Examples of the quaternary ammonium salt having an imidazoline ring include compounds represented by the following general formula (5). These may be used alone or in combination of two or more.
Figure 0005410026
(In the formula, R6 represents an alkyl group having 6 to 24 carbon atoms or an alkenyl group having 6 to 24 carbon atoms, R7 represents an alkyl group having 1 to 24 carbon atoms or an alkenyl group having 1 to 24 carbon atoms, and X -Is an anion.)

本発明において、B成分の疎水部がアルキル基及び/ 又はアルケニル基のときは炭素数が6未満であると十分な界面活性能が得られない場合があり、炭素数が24を超えると分散安定性が悪くなったりする場合がある。したがって、本発明のB成分の炭素数は6〜24の範囲であることが好ましい。   In the present invention, when the hydrophobic part of the component B is an alkyl group and / or alkenyl group, if the carbon number is less than 6, sufficient surface activity may not be obtained. May be worse. Therefore, it is preferable that the carbon number of B component of this invention is the range of 6-24.

上記一般式(5)で表されるイミダゾリン環を有する4級アンモニウム塩としては、具体的な化合物としては1−ヒドロキシエチル−1−エチル−2−オレイルイミダゾリンエチル硫酸塩、1−ヒドロキシエチル−1−メチル−2−オレイルイミダゾリンクロライド、1−ヒドロキシエチル−1−エチル−2−ラウリルイミダゾリンエチル硫酸塩などが挙げられる。   Specific examples of the quaternary ammonium salt having an imidazoline ring represented by the general formula (5) include 1-hydroxyethyl-1-ethyl-2-oleylimidazoline ethyl sulfate, 1-hydroxyethyl-1 -Methyl-2-oleylimidazoline chloride, 1-hydroxyethyl-1-ethyl-2-laurylimidazoline ethyl sulfate and the like.

上記以外のB成分としては、モノメチルエステル4級塩、ジメチルジエステル4級塩、トリメチルジエステル4級塩、エステルアミド型3級塩などが上げられる。
モノメチルエステル4級塩としては、トリエタノールアミンを炭素数7〜25 、好ましくは11〜23の脂肪酸、例えばステアリン酸でジエステル化し、ジメチル硫酸塩で4 級化したものが挙げられ、ジメチルジエステル4級塩としては、N−メチルジエタノールアミンを炭素数7 〜25、好ましくは11〜23の脂肪酸、例えばオレイン酸でジエステル化し、メチルクロライドで4級化したものが挙げられ、トリメチルジエステル4級塩としては、3−ジメチルアミノ−1,2−プロパンジオールを炭素数7〜25、好ましくは11 〜23の脂肪酸、例えばオレイン酸でジエステル化し、メチルクロライドで4級化したものが挙げられ、エステルアミド型3級塩としては、N−(2−ヒドロキシエチル)−N − メチル−1,3−プロパンジアミンを炭素数7〜25、好ましくは11〜23の脂肪酸、例えばオレイン酸でエステル化、アミド化し、塩酸で中和して3 級アンモニウム塩としたものなどが挙げられる。
Examples of the B component other than the above include monomethyl ester quaternary salt, dimethyl diester quaternary salt, trimethyl diester quaternary salt, and ester amide type tertiary salt.
Examples of the monomethyl ester quaternary salt include those obtained by diesterifying triethanolamine with a fatty acid having 7 to 25 carbon atoms, preferably 11 to 23, for example, stearic acid and quaternizing with dimethyl sulfate. Examples of the salt include N-methyldiethanolamine that is diesterified with a fatty acid having 7 to 25 carbon atoms, preferably 11 to 23, for example, oleic acid, and quaternized with methyl chloride. As the trimethyl diester quaternary salt, Examples include 3-dimethylamino-1,2-propanediol, which is diesterified with a fatty acid having 7 to 25 carbon atoms, preferably 11 to 23 carbon atoms, such as oleic acid, and quaternized with methyl chloride. Examples of the salt include N- (2-hydroxyethyl) -N-methyl-1,3-propa Diamine 7-25 carbon atoms, preferably fatty acids of 11 to 23, for example esterified with oleic acid, amidation, and the like those tertiary ammonium salt is neutralized with hydrochloric acid.

本発明におけるA成分とB成分との質量比は、通常、A/B=100/0.5〜100/20であり、好ましくは、A/B=100/2〜100/10である。A成分100重量部に対してB成分が0.5重量部未満であると充分に紙料へ吸着することができない場合があり、またB成分が20 重量部を超えては、その経時安定性が悪くなる場合がある。   The mass ratio of the A component and the B component in the present invention is usually A / B = 100 / 0.5 to 100/20, and preferably A / B = 100/2 to 100/10. If the B component is less than 0.5 parts by weight relative to 100 parts by weight of the A component, it may not be able to be sufficiently adsorbed to the paper stock, and if the B component exceeds 20 parts by weight, its stability over time May get worse.

本発明の柔軟剤は、溶媒中又は無溶媒下に前記A成分及び前記B成分とを含有する。
前記溶媒としては例えば水、イソプロピルアルコール等のアルコール等を挙げることができる。
The softening agent of this invention contains the said A component and the said B component in a solvent or under absence of solvent.
Examples of the solvent include water and alcohols such as isopropyl alcohol.

(柔軟剤定着補助剤)
他方、本発明にかかる柔軟剤定着補助剤は、柔軟剤の定着率を高めるものであり、添加によって基剤紙への柔軟剤の定着率が向上する物質全般を意味する。好適な例としては、ポリアミド・エピクロロヒドリン樹脂を有効成分とするものであり、特には、ポリアミド・エピクロロヒドリン樹脂である。
(Softener fixing aid)
On the other hand, the softener fixing auxiliary agent according to the present invention increases the fixing rate of the softening agent, and means all substances that improve the fixing rate of the softening agent to the base paper when added. Preferable examples include those containing a polyamide / epichlorohydrin resin as an active ingredient, and particularly a polyamide / epichlorohydrin resin.

この柔軟剤定着補助剤は、有効成分を固形分で0.1〜2.5kg/t含むように調整するのが望ましい。また、柔軟剤定着補助剤は、イオン的に両性であるのが望ましく、カチオン性、アニオン性、ノニオン性であると十分な効果が得られないことがある。   This softener fixing auxiliary agent is preferably adjusted so that the active ingredient is contained in a solid content of 0.1 to 2.5 kg / t. Further, the softener fixing auxiliary agent is desirably ionic amphoteric, and if it is cationic, anionic, or nonionic, sufficient effects may not be obtained.

柔軟剤定着補助剤の使用にあたっては、水等の水性溶媒を用い、粘度調整剤、pH調整剤等を適宜用い、適宜使用に適す粘度等に調整する。   In using the softener fixing auxiliary agent, an aqueous solvent such as water is used, and a viscosity adjusting agent, a pH adjusting agent, or the like is used as appropriate, and the viscosity is adjusted to be suitable for use.

前記ポリアミド・エピクロロヒドリン樹脂を用いるのであれば、好ましくその分子量が10万以上100万以下であり、特に60万以下が望ましい。分子量が10万以下であると添加した際の定着性が悪く、100万を超えると紙力を高める効果が強く発現し、抄造後の紙の風合い悪化を招く。   If the polyamide / epichlorohydrin resin is used, the molecular weight is preferably 100,000 or more and 1,000,000 or less, particularly preferably 600,000 or less. When the molecular weight is 100,000 or less, the fixing property when added is poor, and when it exceeds 1,000,000, the effect of increasing paper strength is strongly expressed, and the paper texture after papermaking is deteriorated.

柔軟剤に加えてこの柔軟剤定着補助剤を併用することで、前記柔軟剤の基材紙への定着率が向上し、紙力の低下なく柔らかさが向上し、さらに滑らかさも向上する。   By using this softener fixing auxiliary in addition to the softener, the fixing ratio of the softener to the base paper is improved, the softness is improved without a decrease in paper strength, and the smoothness is also improved.

(配合割合)
他方、前記薄葉紙処理剤における柔軟剤と柔軟剤定着補助剤との配合割合は、少なくとも柔軟剤が質量割合で多く含み、好ましくは、質量比で、柔軟剤:柔軟剤定着補助剤=2.8:2.5から10:1である。柔軟剤に対して柔軟助剤の量が少ないと、基材紙への定着率が十分でなく、柔らかさと滑らかさが十分に発現しない。柔軟剤定着補助剤の量が多いと、紙力が高まりすぎて、風合い悪化を招く恐れがある。
(Mixing ratio)
On the other hand, the blending ratio of the softening agent and the softening agent fixing auxiliary agent in the thin paper treatment agent includes at least the softening agent in a mass ratio, and preferably, the softening agent: softening agent fixing auxiliary agent = 2.8 by mass ratio. : 2.5 to 10: 1. When the amount of the softening aid is small relative to the softening agent, the fixing rate to the base paper is not sufficient, and the softness and smoothness are not sufficiently exhibited. When the amount of the softener fixing auxiliary agent is large, the paper strength is excessively increased, and the texture may be deteriorated.

(含有量等)
他方、本発明の衛生用薄葉紙においては、前記柔軟剤の含有量が、0.1〜2.8kg/tであることが望ましい。0.1kg/t未満であると、柔軟性、滑らかさ、紙力の発現が十分ではなく、2.8kg/tを超えると、拭き取りに必要な紙力を確保することが難しく、パルプの叩解や米坪を増やす等の処置が必要となる。その結果、風合いが硬くなる傾向にある。なお、この含有量は、上記柔軟剤定着補助剤の併用により確実に達成可能である。
(Content etc.)
On the other hand, in the sanitary thin paper of the present invention, it is desirable that the content of the softening agent is 0.1 to 2.8 kg / t. If it is less than 0.1 kg / t, the expression of flexibility, smoothness, and paper strength is not sufficient, and if it exceeds 2.8 kg / t, it is difficult to secure the paper strength necessary for wiping. It is necessary to take measures such as increasing the floor area. As a result, the texture tends to be hard. This content can be reliably achieved by the combined use of the softening agent fixing aid.

他方、本発明の薄葉紙処理剤は、抄紙原料( パルプスラリー) に添加して使用してもよく、原紙の表面に塗工して( 即ち、表面塗工して) 使用しても良い。   On the other hand, the thin paper treating agent of the present invention may be used by adding to a papermaking raw material (pulp slurry), or may be used by coating on the surface of the base paper (that is, coating the surface).

上記本発明の薄葉紙処理剤は、その薄葉紙処理剤中の柔軟剤の基材紙への定着率が80質量%を超え、従来の60質量%程度と比較して、極めて高くすることができるから、これを考慮して、その添加量を定める。   The thin paper treating agent of the present invention has a fixing ratio of the softening agent in the thin paper treating agent to the base paper exceeding 80% by mass, and can be extremely high as compared with the conventional about 60% by mass. In consideration of this, the addition amount is determined.

更に、本発明の薄葉紙処理剤を抄紙原料に添加し、次いで抄紙し、乾燥して得られた原紙の表面に本発明の薄葉紙処理剤をさらに塗工するようにしてもよい。
本発明の薄葉紙処理剤を抄紙原料に添加して使用する場合、その使用方法は特に制限はなく、工業水などにより希釈して添加することもでき、そのまま添加することもできる。
Furthermore, the thin paper treating agent of the present invention may be further applied to the surface of the base paper obtained by adding the thin paper treating agent of the present invention to the papermaking raw material, then papermaking and drying.
When the thin paper treating agent of the present invention is used by adding it to the papermaking raw material, the method of use is not particularly limited, and it can be diluted with industrial water or the like, or can be added as it is.

いずれの場合も、一般的な紙の製造方法と同様の方法を採用できる。
他方、本発明の紙用柔軟剤を表面塗工に適用する好ましい方法としては、スプレー法による塗工、フレキソ法又はグラビア法による印刷機による塗工、サイズプレス、ゲートロールコーター、ビルブレードコーター又はカレンダーなどでの塗工などが挙げられるが、いずれの場合も、本発明の紙用柔軟剤を用いること以外は、一般的な紙の製造方法と同様の方法を採用できる。
In any case, a method similar to a general paper manufacturing method can be adopted.
On the other hand, preferred methods for applying the paper softener of the present invention to surface coating include spray coating, flexo printing or gravure printing using a printing press, size press, gate roll coater, bill blade coater or Examples include coating with a calender and the like. In any case, a method similar to a general paper manufacturing method can be adopted except that the paper softener of the present invention is used.

〔衛生用薄葉紙の構造・物性等〕
他方、本発明の衛生用薄葉紙の構造は、基材紙に応じて1プライであっても、2プライ(2枚重ねで一組)、3プライ、4プライ又はそれ以上の複数プライであってもよい。複数プライとする場合、表面を構成する基材紙のみに薬液が含有されていても、全ての基材紙に薬液が含有されていてもよい。
[Structure and physical properties of sanitary thin paper]
On the other hand, the structure of the sanitary thin paper of the present invention may be 1 ply according to the base paper, 2 plies (a set of two stacked sheets), 3 plies, 4 plies or more plies. Also good. In the case of a plurality of plies, the chemical solution may be contained only in the base paper constituting the surface, or the chemical solution may be contained in all the base papers.

また、本発明の衛生用薄葉紙は、特にトイレットペーパー、ティシュペーパーに適しており、この用途に用いるのがよい。本発明の効果を実感しやすい。   In addition, the sanitary thin paper of the present invention is particularly suitable for toilet paper and tissue paper, and is preferably used for this purpose. It is easy to feel the effect of the present invention.

他方、本発明の衛生用薄葉紙は、その伸び率が7〜15%であるのが好ましい。特に好ましくは8〜13%である。伸び率が7%未満であると製造時に破れ、断紙等のトラブルが発生する。また、伸び率が15%を超える紙はクレープ率を高めるなど紙表面の凹凸の数を多くする必要があり、肌を擦った時にざらつきを感じるものとなるため好ましくない。   On the other hand, the sanitary thin paper of the present invention preferably has an elongation of 7 to 15%. Most preferably, it is 8 to 13%. If the elongation is less than 7%, it is torn during production and troubles such as paper breakage occur. Also, paper with an elongation of more than 15% is not preferable because it needs to increase the number of irregularities on the surface of the paper such as increasing the crepe rate, and feels rough when rubbing the skin.

この伸び率は、JIS P 8113に準じて測定する。具体的には、紙の縦方向の乾燥引張強度を測定し、その破断直前の紙の長さと測定前の紙の長さとから、紙の伸び率を算出する。測定は最終製品、すなわち2プライの製品であれば2プライで、3プライの製品であれば3プライにて測定を行う。   This elongation rate is measured according to JIS P8113. Specifically, the dry tensile strength in the machine direction of the paper is measured, and the elongation percentage of the paper is calculated from the length of the paper immediately before the break and the length of the paper before the measurement. The measurement is performed with 2 plies for the final product, that is, a 2-ply product, and with 3 plies for a 3-ply product.

なお伸び率は、クレープ率との相関が大きく、当該伸び率を好適に達成するために、基材紙の製造時のクレープ率を12.0〜20.0%にするのが望ましい。なお、クレープ率は、式(((製紙時のドライヤーの周速)−(リール周速))/(製紙時のドライヤーの周速)×100)により算出される値である。   The elongation rate has a large correlation with the crepe rate, and in order to suitably achieve the elongation rate, it is desirable that the crepe rate at the time of manufacturing the base paper is 12.0 to 20.0%. The crepe rate is a value calculated by the formula (((peripheral speed of the dryer during paper manufacture) − (peripheral speed of the reel)) / (peripheral speed of the dryer during paper manufacture) × 100).

他方、本発明の衛生用薄葉紙は、JIS P 8113に規定される乾燥引張強度(以下、乾燥紙力ともいう)が、縦方向200〜350cN/25mm、より好ましくは200〜300cN/25mm、横方向90〜140cN/25mmであるのが好ましい。乾燥紙力が低過ぎると、製造時に破れ、断紙等のトラブルが発生し易くなり、高過ぎると使用時にごわごわした肌触りとなる。
これらの乾燥紙力は、本発明においては、乾燥紙力剤の必要なく達成できる。従って、本発明の衛生用薄葉紙においては乾燥紙力剤を含有しないほうが好ましい。
On the other hand, the sanitary thin paper of the present invention has a dry tensile strength (hereinafter also referred to as dry paper strength) specified in JIS P 8113 of 200 to 350 cN / 25 mm in the longitudinal direction, more preferably 200 to 300 cN / 25 mm, and transverse direction. It is preferably 90 to 140 cN / 25 mm. If the dry paper strength is too low, it tends to break during manufacturing and troubles such as paper breakage occur, and if it is too high, the touch becomes stiff when used.
These dry paper strengths can be achieved in the present invention without the need for dry paper strength agents. Therefore, it is preferable that the sanitary thin paper of the present invention does not contain a dry paper strength agent.

用いないとされる乾燥紙力剤には、澱粉、カチオン性澱粉、カチオン性変成澱粉、CMC(カルボキシメチルセルロース)若しくはその塩であるカルボキシメチルセルロースナトリウム、カルボキシメチルセルロースカルシウム、カルボキシメチルセルロース亜鉛が含まれる。少なくとも、ここに掲げるものは含有されない。   Dry paper strength agents that are not used include starch, cationic starch, cationic modified starch, carboxymethylcellulose sodium, carboxymethylcellulose calcium, and carboxymethylcellulose zinc, which are CMC (carboxymethylcellulose) or salts thereof. At least those listed here are not included.

他方、本発明の衛生用薄葉紙の紙厚(尾崎製作所製ピーコックにより測定)は、例えば2プライ(2枚重ね)で100〜300μm、特に110〜200μmであるのが好ましく、1プライの場合はその半分であるのが望ましい。   On the other hand, the paper thickness of the sanitary thin paper of the present invention (measured by a Peacock manufactured by Ozaki Seisakusho) is preferably 100 to 300 μm, particularly 110 to 200 μm, preferably 2 plies (two sheets stacked), It is desirable to be half.

他方、本発明の衛生用薄葉紙は、MMDの値が7〜8.5であるのが望ましい。なお、ここでのMMDは、JIS P 8111に規定される条件下で測定した、摩擦係数の平均偏差MMDである。摩擦係数の平均偏差MMDは、カトーテック株式会社製「摩擦感テスター KES SE」を用いて測定することができる。MMD値が大きいほど滑らかさに劣ることを意味する。   On the other hand, it is desirable that the sanitary thin paper of the present invention has an MMD value of 7 to 8.5. In addition, MMD here is the average deviation MMD of a friction coefficient measured on the conditions prescribed | regulated to JISP8111. The average deviation MMD of the friction coefficient can be measured using “Friction Sense Tester KES SE” manufactured by Kato Tech Co., Ltd. A larger MMD value means less smoothness.

他方、本発明の衛生用薄葉紙は、MMDに基づく肌触り試験の値が8.5〜10.0であるのが望ましい。この肌触り試験は、通常のMMD試験機、例えば、図1〜図3に示すように、カトーテック株式会社製の摩擦感テスター「KES SE」の基台上に人工皮革(サプラーレ:出光テクノファイン社製)を敷いて固定するとともに、測定端子を人工皮革(サプラーレ:出光テクノファイン社製)にて被覆し、その測定端子の測定面の人工皮革で被覆し、MMDの測定手順と同様にして行なう。この肌触り試験は、実際に肌に触れたときに感じる滑らかさに相関する。   On the other hand, the sanitary thin paper of the present invention desirably has a touch test value based on MMD of 8.5 to 10.0. This touch test is performed by using an artificial leather (supplement: Idemitsu Techno Fine Co., Ltd.) on a base of a normal MMD tester, for example, a friction tester “KES SE” manufactured by Kato Tech Co., Ltd. as shown in FIGS. The measurement terminal is covered with artificial leather (Supplar: manufactured by Idemitsu Techno Fine Co., Ltd.), and the measurement surface of the measurement terminal is covered with artificial leather, and this is performed in the same manner as the MMD measurement procedure. . This touch test correlates with the smoothness felt when actually touching the skin.

測定の詳細を更に説明すると、人工皮革で構成される接触平面は、ほぼ10mm四方の測定面を有するシリコン製のMMD測定用端子を、前記人工皮革で被覆して形成する。   The details of the measurement will be further described. The contact plane made of artificial leather is formed by covering a silicon MMD measurement terminal having a measurement surface of approximately 10 mm square with the artificial leather.

そして人工皮革による前記端子の被覆は、10mm四方の接触平面が形成されるように端子の測定面に対して人工皮革がぴったりと接触するように、あるいは若干の張力をもたせてぴったりと被覆することにより達成することができる。人工皮革を端子に固定するにあたっては、測定時、すなわち紙試料を移動させたときに人工皮革と内部の端子とがずれて人工皮革や接触平面に歪みなどが生じないようにしっかりと固定することが重要である。固定は、例えば、前記接触平面が構成されるように前記端子を被覆したのち、接触平面を構成しない部位を輪ゴム等で装置の測定に影響が出ない部位、例えば端子の支持材等にしっかり固定する。また、MMD試験機の基台上には人工皮革を敷いて接着テープ等で固定する。このとき、測定時に歪まないように基台に人工皮革をしっかりと固定することが重要である。また、基台上に敷く人工皮革は、前記接触平面を構成する人工皮革と同じものを用いる。なお、紙試料は、10cm四方に裁断して用い、人工皮革を敷いた基台に固定する。測定に際しては、紙試料の上に試料押さえ用錘(約100g)で押さえる。また、試験機の測定端子への荷重を15gとして行う。測定は、紙試料の縦方向について3回、横方向について3回の計6回を行い、測定値(KES肌触り指数)についてはその6回の平均値とする。また、紙試料は、2プライを原則として、1プライを想定する場合には試料を2枚重ねにして測定する。本試験においては6回の平均値を10倍したものを肌触り試験値として採用した。
以上詳述の本発明の衛生用薄葉紙は、紙力の低下なく、また、滑らかさと柔らかさが従来例と比較して十分に向上され、使用において優れた利点を有する。
The terminal is covered with artificial leather so that the artificial leather is in close contact with the measurement surface of the terminal so that a 10 mm square contact plane is formed, or with a slight tension. Can be achieved. When fixing the artificial leather to the terminal, make sure that the artificial leather and the internal terminal are not displaced when measuring, that is, when the paper sample is moved, so that the artificial leather and the contact plane are not distorted. is important. For example, after covering the terminal so that the contact plane is configured, the part that does not configure the contact plane is securely fixed to a part that does not affect the measurement of the device with a rubber band or the like, such as a support material for the terminal. To do. Also, artificial leather is laid on the base of the MMD testing machine and fixed with adhesive tape or the like. At this time, it is important to firmly fix the artificial leather to the base so as not to be distorted during measurement. The artificial leather laid on the base is the same as the artificial leather constituting the contact plane. In addition, the paper sample is cut into a 10 cm square and used, and is fixed to a base on which artificial leather is laid. At the time of measurement, a sample pressing weight (about 100 g) is pressed on a paper sample. Moreover, the load to the measurement terminal of a testing machine is performed as 15g. The measurement is performed three times in the vertical direction of the paper sample and three times in the horizontal direction for a total of six times, and the measured value (KES feel index) is the average value of the six times. In addition, in principle, two plies are used for a paper sample, and when one ply is assumed, two samples are stacked and measured. In this test, the average value of 6 times 10 times was adopted as the touch test value.
The sanitary thin paper of the present invention described above in detail has no advantage in paper strength, smoothness and softness are sufficiently improved as compared with conventional examples, and has excellent advantages in use.

次いで、その本発明の実施例と比較例との柔らかさなどについて試験した結果を実施例として以下に示す。   Subsequently, the result of having tested about the softness etc. of the Example of this invention and a comparative example is shown below as an Example.

下記表1〜表4は、本願発明の実施例及び比較例にかかる衛生用薄葉紙の組成・物性を測定した結果及び各例について官能評価の結果を示したものである。   The following Tables 1 to 4 show the results of measuring the composition and physical properties of sanitary thin papers according to Examples and Comparative Examples of the present invention and the results of sensory evaluation for each example.

Figure 0005410026
Figure 0005410026

Figure 0005410026
Figure 0005410026

Figure 0005410026
Figure 0005410026

Figure 0005410026
Figure 0005410026

なお、官能評価については以下のように行った
「柔らかさ」
被験者30人の官能評価とした。評価は、試料となる薄葉紙を触る、顔にあてる、鼻をかむ等して柔らかさについて、どのように感じるかを基準例を基準として、点数付けすることで行った。点数は、1点:基準例と比べると明らかに風合いの劣ることがわかる、2点:基準例と比べると風合いが若干劣ることがわかる、3点:基準例比較例1と同等、4点:基準例と比べると若干風合いが勝ることがわかる、5点:基準例と比べると明らかに風合いの勝ることがわかる。表中の点数は30人の平均である。
The sensory evaluation was performed as follows: “Softness”
A sensory evaluation of 30 subjects was performed. The evaluation was performed by scoring how the soft paper felt by touching the thin paper as a sample, hitting the face, biting the nose, etc. based on the reference example. The score is 1 point: the texture is clearly inferior to the reference example, 2 points: the texture is slightly inferior to the reference example, 3 points: the same as the reference example comparative example 1, 4 points: It can be seen that the texture is slightly better than the reference example. 5 points: It is clearly understood that the texture is superior to the reference example. The score in the table is the average of 30 people.

「滑らかさ」
被験者30人の官能評価とした。評価は、試料となる薄葉紙を触る、顔にあてる、鼻をかむ等して滑らかさについて、どのように感じるかを基準例を基準として、点数付けすることで行った。点数は、1点:基準例と比べると明らかに風合いの劣ることがわかる、2点:基準例と比べると風合いが若干劣ることがわかる、3点:基準例と同等、4点:基準例と比べると若干風合いが勝ることがわかる、5点:基準例と比べると明らかに風合いの勝ることがわかる。表中の点数は30人の平均である。
"Smoothness"
A sensory evaluation of 30 subjects was performed. The evaluation was performed by scoring how to feel the smoothness by touching the thin paper as a sample, hitting the face, biting the nose, etc., based on the reference example. The score is 1 point: the texture is clearly inferior to the reference example, 2 points: the texture is slightly inferior to the reference example, 3 points: the same as the reference example, 4 points: the reference example It can be seen that the texture is slightly superior when compared, 5 points: The texture is clearly superior when compared with the reference example. The score in the table is the average of 30 people.

「ふんわり感」
被験者30人の官能評価とした。評価は、試料となる薄葉紙を触る、顔にあてる、鼻をかむ等してふんわり感について、どのように感じるかを基準例を基準として、点数付けすることで行った。点数は、1点:基準例と比べると明らかに風合いの劣ることがわかる、2点:基準例と比べると風合いが若干劣ることがわかる、3点:基準例と同等、4点:基準例と比べると若干風合いが勝ることがわかる、5点:基準例と比べると明らかに風合いの勝ることがわかる。表中の点数は30人の平均である。
"Soft feeling"
A sensory evaluation of 30 subjects was performed. The evaluation was performed by scoring how the soft paper feels by touching the thin paper as a sample, hitting the face, biting the nose, etc., based on the reference example. The score is 1 point: the texture is clearly inferior to the reference example, 2 points: the texture is slightly inferior to the reference example, 3 points: the same as the reference example, 4 points: the reference example It can be seen that the texture is slightly superior when compared, 5 points: The texture is clearly superior when compared with the reference example. The score in the table is the average of 30 people.

なお、各官能評価における基準例とは、表中においてすべての官能評価値が3.0となっているものである。
また、薄葉紙処理剤における、柔軟剤は、T−FS301(星光PMC株式会社製)及びこれの主成分分子量を調製したものを用いた。また、柔軟剤定着補助剤は、T−FS371(星光PMC株式会社製)を用い、抄紙原料に対して内添して用いた。また、澱粉はDD−4280(星光PMC株式会社製)を用いた。
また、各試験にかかる測定方法は、上記詳細な説明にて説明した測定方法に従い、ソフトネスは、JIS L1096 E法に準じたハンドルオメータ法に基づいて測定した。
In addition, the reference examples in each sensory evaluation are those in which all sensory evaluation values are 3.0 in the table.
Moreover, what prepared the T-FS301 (made by Seiko PMC Co., Ltd.) and the main component molecular weight was used for the softening agent in a thin paper processing agent. Further, T-FS371 (manufactured by Seiko PMC Co., Ltd.) was used as the softener fixing auxiliary agent, and was used by being internally added to the papermaking raw material. Moreover, DD-4280 (made by Seiko PMC Co., Ltd.) was used as the starch.
Moreover, the measuring method concerning each test followed the measuring method demonstrated in the said detailed description, and softness was measured based on the handle ohm method according to JISL1096E method.

表1は、本願発明の主に柔軟剤及び柔軟剤定着補助剤の効果を確認した試験の結果である。表1より、本願発明にかかる実施例11〜13より、滑らかさの指標となるMMDの値が7.7未満であり、同様に滑らかさ試験の数値も9.4、柔らかさの指標となるソフトネスは1.7未満であり、ふんわり感の指標となる紙厚は135μm以上である。使用において十分な値である。
なお、実施例11及び12は柔軟剤定着補助剤の添加量比率を変更している。また、実施例13は乾燥紙力増強剤として澱粉を添加している。
Table 1 shows the results of a test for confirming the effects of the softener and the softener fixing auxiliary agent of the present invention. From Table 11, from Examples 11 to 13 according to the present invention, the value of MMD which is an index of smoothness is less than 7.7, and the numerical value of the smoothness test is also 9.4, which is an index of softness. The softness is less than 1.7, and the paper thickness serving as an index of soft feeling is 135 μm or more. Sufficient value in use.
In Examples 11 and 12, the addition ratio of the softener fixing auxiliary agent is changed. In Example 13, starch was added as a dry paper strength enhancer.

試験の結果、本発明の実施例は、柔軟剤のみの添加及び柔軟剤未添加である比較例11及び12よりも、官能評価及び滑らかさ、ソフトネスにおいて高い評価であることが確認できた。   As a result of the test, it was confirmed that the examples of the present invention were higher in sensory evaluation, smoothness, and softness than Comparative Examples 11 and 12 in which only the softener was added and no softener was added.

なお、実施例11と12とでは、実施例11の方が柔軟剤定着補助剤の添加量がより望ましい値であることが確認できる。
また、実施例14及び15は実施例1からクレープ率の変更を行った例である。その結果、クレープ率を下げることにより滑らかさ、肌触りの良さは向上し、クレープ率を上げることで滑らかさ、肌触りの良さは低下することが確認できた。これはクレープ率を下げることで紙の表面の凹凸が少なくなるために起こったことと推測する。従って、当該クレープ率についても、適宜の範囲とするのが望ましい。
In Examples 11 and 12, it can be confirmed that Example 11 has a more desirable value for the addition amount of the softener fixing auxiliary.
Examples 14 and 15 are examples in which the crepe rate was changed from Example 1. As a result, it was confirmed that lowering the crepe rate improved the smoothness and feel, and increasing the crepe rate reduced the smoothness and feel. This is presumed to have occurred because the unevenness of the paper surface was reduced by lowering the crepe rate. Therefore, it is desirable that the crepe rate is within an appropriate range.

他方、実施例11〜15からは、柔軟剤定着補助剤を添加することにより柔軟剤の定着量が向上することが理解できる。本願発明にかかる柔軟剤及び柔軟剤定着補助剤を用いることで、柔軟剤の定着率が向上することが確認できた。   On the other hand, it can be understood from Examples 11 to 15 that the amount of fixing of the softening agent is improved by adding the softening agent fixing auxiliary agent. It has been confirmed that the use of the softening agent and softening agent fixing auxiliary agent according to the present invention improves the fixing rate of the softening agent.

また、比較例13は、柔軟剤及び柔軟剤定着補助剤とを含有させたものであるが、柔軟剤よりも柔軟剤定着補助剤の量が多いものである。結果をみてみると、柔軟剤の定着量は向上しているものの、ソフトネス、紙厚の値が低下している。結果から、柔軟剤定着補助剤の添加量が柔軟剤よりも多くなると、柔軟剤の効果が柔軟剤定着補助剤自体の有する表面性を低下させる効果が勝り、良好な結果が発揮されないと推測される。   Comparative Example 13 contains a softening agent and a softening agent fixing auxiliary agent. However, the amount of the softening agent fixing auxiliary agent is larger than that of the softening agent. As a result, although the fixing amount of the softening agent has improved, the values of softness and paper thickness have decreased. From the results, it is presumed that when the amount of the softener fixing auxiliary added is larger than that of the softener, the effect of the softener is superior in reducing the surface properties of the softener fixing auxiliary itself, and good results are not exhibited. The

他方、表2は、主に柔軟剤定着補助剤の分子量の相違について検討を行った結果である。官能評価については比較例20を基準例として評価を実施した。表2から、実施例20〜22に関しては、滑らかさの指標となるMMDの値が7.9未満であり、同様に滑らかさ試験の数値も9.4柔らかさの指標となるソフトネスは1.65未満であり、ふんわり感の指標となる紙厚は137μm以上であり、良好な結果となっている。十分に良好な結果が得られた。
実施例23、24は数値的に大きな向上が見られなかった。
On the other hand, Table 2 shows the results of studies on differences in molecular weights of softener fixing aids. The sensory evaluation was carried out using Comparative Example 20 as a reference example. From Table 2, with respect to Examples 20 to 22, the value of MMD, which is an index of smoothness, is less than 7.9, and similarly, the numerical value of the smoothness test is also 1 for softness, which is an index of 9.4 softness. It is less than .65, and the paper thickness, which is an index of soft feeling, is 137 μm or more, which is a good result. Good enough results were obtained.
In Examples 23 and 24, no significant improvement in numerical value was observed.

上記の結果より、23の場合は柔軟剤定着補助剤の分子量が少ないことから実施例20程の柔軟剤定着量が見られないため数値の改善が見られなかったと推測する。また実施例24については柔軟剤定着補助剤の分子量が多いことから柔軟剤の定着剤としての効果は見られるものの、接着性が発現したことから紙厚、ソフトネスの向上が見られなかったと推測する。   From the above results, in the case of 23, the molecular weight of the softening agent fixing auxiliary agent is small, so that the softening agent fixing amount as in Example 20 is not seen, so it is presumed that the numerical value was not improved. In Example 24, since the softener fixing auxiliary agent has a large molecular weight, the effect of the softener as a fixing agent can be seen. However, since the adhesiveness was developed, it was estimated that the paper thickness and softness were not improved. To do.

表3では、柔軟剤の添加量について検討を行った。実施例30、比較例31、32より、柔軟剤添加量を変化させることで品質が大きく変化していることがわかる。比較例32については比較例31よりも柔軟剤定着量が多く、MMD、滑らかさ試験、紙厚、ソフトネスの数値は若干改善の傾向にある。しかしその効果は柔軟剤の定着量の多い実施例30に及ばない。従って、本願発明の柔軟剤の定着により柔軟性が高まることが確認できた。   In Table 3, the addition amount of the softening agent was examined. From Example 30 and Comparative Examples 31 and 32, it can be seen that the quality greatly changes by changing the softener addition amount. In Comparative Example 32, the softener fixing amount is larger than in Comparative Example 31, and the numerical values of MMD, smoothness test, paper thickness, and softness tend to be slightly improved. However, the effect does not reach Example 30 where the fixing amount of the softening agent is large. Therefore, it was confirmed that the flexibility was increased by fixing the softener of the present invention.

また、比較例33及び34は実施例31から柔軟剤を増添加した結果、紙力を維持できないため抄造することができなかった。澱粉の添加や叩解等での紙力調整は行えるが、柔らかさ、紙厚等の数値が好適な範囲を維持できないため実施しなかった。   In Comparative Examples 33 and 34, as a result of adding the softening agent from Example 31, paper strength could not be maintained and papermaking could not be performed. Although the paper strength can be adjusted by adding starch, beating, etc., it was not carried out because numerical values such as softness and paper thickness could not be maintained within a suitable range.

表4は、操業性に関しての試験を行った。主に、対象となる薄葉紙(原紙シート)の米坪及びクレープ率についての検討である。表4から、過度に低い坪量、また高い坪量は本願発明の薄葉紙として適さないことが確認できた。具体的には、米坪に関しては少なくとも9g/m2以下、27g/m2以上であると操業が困難となることがあり、また、クレープ率が12であると同様に操業が困難になることがあることが確認できた。従って、当該範囲を考慮して、本願発明にかかる薄葉紙(原紙シート)を設計するのが望ましい。 Table 4 tested the operability. Mainly, it is a study on the tsubo and crepe rate of the target thin paper (base paper sheet). From Table 4, it was confirmed that an excessively low basis weight and a high basis weight are not suitable as the thin paper of the present invention. Specifically, with respect to rice tsubo, at least 9 g / m 2 or less and 27 g / m 2 or more, the operation may be difficult, and if the crepe rate is 12, the operation may be difficult. It was confirmed that there is. Therefore, it is desirable to design the thin paper (base paper sheet) according to the present invention in consideration of the range.

以上の表1〜4に示される結果を総合すれば、本願発明にかかる衛生用薄葉紙は、柔らかさ及び滑らかさに優れており、しかも、操業上のトラブルなく製造でき、さらに紙力も十分であるといえる。   Summarizing the results shown in Tables 1 to 4 above, the sanitary thin paper according to the present invention is excellent in softness and smoothness, can be produced without any operational trouble, and has sufficient paper strength. It can be said.

本発明は、ティシュペーパー、トイレットペーパー、キッチンペーパー、クレープ紙等の衛生用薄葉紙に適用可能なものである。   The present invention is applicable to sanitary thin paper such as tissue paper, toilet paper, kitchen paper, and crepe paper.

MMDに基づく肌触り試験を説明するための第1の図である。It is a 1st figure for demonstrating the touch test based on MMD. MMDに基づく肌触り試験を説明するための第2の図である。It is a 2nd figure for demonstrating the touch test based on MMD. MMDに基づく肌触り試験を説明するための第3の図である。It is a 3rd figure for demonstrating the touch test based on MMD.

X1…MMDに基づく肌触り試験を行うための試験機   X1 ... Testing machine for MMD-based touch test

Claims (1)

基材紙に対して薄葉紙処理剤を含有させた衛生用薄葉紙であって、
前記薄葉紙処理剤が柔軟剤と柔軟剤定着補助剤とを含み、
前記柔軟剤が、
アルキル基及び/又はアルケニル基を有する非イオン性界面活性剤(A成分)とアルキル基及び/又はアルケニル基を有するカチオン性界面活性剤(B成分)とを含有し、それらの固形分重量比がA成分/B成分=100/0.5〜100/20であり、
前記A成分が下記一般式(1)、(2)及び(3)で表される化合物の少なくとも一種であり、
1−A1−(EO)m(PO)n−CO−R2 ・・・(1)
1−O−(EO)m(PO)n−R2 ・・・(2)
1−A1−(EO)m(PO)nH ・・・(3)
(但し、式中、−A1−は−O−又は−COO−を示し、R1とR2とは炭素数6〜24のアルキル基又は炭素数6〜24のアルケニル基を示し、かつR1とR2とは同一又は相異してもよく、Eはエチレン基を示し、Pはプロピレン基を示し、mとnとの合計は1〜60である。なお、m及びnは平均付加モル数である。)
前記B成分がアルキル基及び/又はアルケニル基を有するイミダゾリン環を有する4級アンモニウム塩、又は下記一般式(4)で表される化合物であり、
Figure 0005410026
前記柔軟剤定着補助剤が、
ポリアミド・エピクロロヒドリン樹脂であり、
前記柔軟剤と柔軟剤定着補助剤の質量比が2.8:2.5〜10:1であり、
かつ、柔軟剤の含有量が0.7〜2.8kg/tであり、柔軟剤定着補助剤の含有量が0.1〜2.5kg/tであり、
JIS P 8113に規定される乾燥引張強度が、縦方向200〜350cN/25mm、横方向90〜140cN/25mmであり、かつ、
澱粉、カチオン性澱粉、カチオン性変成澱粉、カルボキシメチルセルロース若しくはその塩であるカルボキシメチルセルロースナトリウム、カルボキシメチルセルロースカルシウム、カルボキシメチルセルロース亜鉛が含有されていない、
ことを特徴とする衛生用薄葉紙。
A sanitary thin paper containing a thin paper treating agent for a base paper,
The tissue paper treating agent includes a softening agent and a softening agent fixing aid,
The softener is
A nonionic surfactant having an alkyl group and / or alkenyl group (component A) and a cationic surfactant having an alkyl group and / or alkenyl group (component B), and the solid content weight ratio thereof is A component / B component = 100 / 0.5 to 100/20,
The component A is at least one compound represented by the following general formulas (1), (2) and (3),
R 1 -A 1- (EO) m (PO) n -CO-R 2 (1)
R 1 —O— (EO) m (PO) n —R 2 (2)
R 1 -A 1- (EO) m (PO) n H (3)
(In the formula, —A 1 — represents —O— or —COO—, R 1 and R 2 represent an alkyl group having 6 to 24 carbon atoms or an alkenyl group having 6 to 24 carbon atoms, and R 1 and R 2 may be the same or different, E represents an ethylene group, P represents a propylene group, and the sum of m and n is 1 to 60, where m and n are average additions Number of moles.)
The B component is a quaternary ammonium salt having an imidazoline ring having an alkyl group and / or an alkenyl group, or a compound represented by the following general formula (4):
Figure 0005410026
The softener fixing auxiliary agent is
A polyamide / epichlorohydrin resin,
The mass ratio of the softener and softener fixing aid is 2.8: 2.5-10: 1;
And content of a softening agent is 0.7-2 . 8 kg / t, the content of the softener fixing auxiliary is 0.1 to 2.5 kg / t,
The dry tensile strength defined in JIS P 8113 is 200 to 350 cN / 25 mm in the longitudinal direction, 90 to 140 cN / 25 mm in the transverse direction, and
Contains no starch, cationic starch, cationic modified starch, carboxymethylcellulose or its salt, carboxymethylcellulose sodium, carboxymethylcellulose calcium, carboxymethylcellulose zinc,
Hygienic thin paper characterized by that.
JP2008068292A 2008-03-17 2008-03-17 Sanitary tissue paper Active JP5410026B2 (en)