JP3048704B2 - Continuous pickling method for steel strip - Google Patents

Continuous pickling method for steel strip

Info

Publication number
JP3048704B2
JP3048704B2 JP3263140A JP26314091A JP3048704B2 JP 3048704 B2 JP3048704 B2 JP 3048704B2 JP 3263140 A JP3263140 A JP 3263140A JP 26314091 A JP26314091 A JP 26314091A JP 3048704 B2 JP3048704 B2 JP 3048704B2
Authority
JP
Japan
Prior art keywords
steel strip
pickling
yellow
rust
continuous
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP3263140A
Other languages
Japanese (ja)
Other versions
JPH05140773A (en
Inventor
彦作 松永
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
JFE Steel Corp
Original Assignee
JFE Steel Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by JFE Steel Corp filed Critical JFE Steel Corp
Priority to JP3263140A priority Critical patent/JP3048704B2/en
Publication of JPH05140773A publication Critical patent/JPH05140773A/en
Application granted granted Critical
Publication of JP3048704B2 publication Critical patent/JP3048704B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Description

【発明の詳細な説明】DETAILED DESCRIPTION OF THE INVENTION

【0001】[0001]

【産業上の利用分野】本発明は鋼帯の連続酸洗付加方法
に係り、特に連続酸洗終了時の低速通板域もしくは通板
停止時に発生する鋼板表面上の錆もしくは黄変色を除去
する簡易付加方法に関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a method for adding a continuous pickling of a steel strip, and more particularly to a method for removing rust or yellow discoloration on a steel sheet surface generated at the time of a low speed passing area at the end of the continuous pickling or at the time of stopping the passing. It relates to a simple addition method.

【0002】[0002]

【従来の技術】熱間圧延後の鋼帯は、表面に付着する酸
化鉄を除去するために連続酸洗ラインに通板する。しか
しながら、この連続通板ライン末期の低速通板域もしく
は通板停止時に鋼板の端部が黄変色になることが往々に
してあり、製品品質上問題となつている。これらの黄変
色は一種の錆であって、酸洗によって鋼帯表面のスケー
ルが除去された地鉄が水と空気中の酸素との化合により
発生するか、もしくは酸洗後の鋼帯表面に付着した鉄塩
が、酸素と十分な水が存在するところで反応して水酸化
第2鉄を生じること等によって発生するものである。
2. Description of the Related Art A steel strip after hot rolling is passed through a continuous pickling line to remove iron oxide adhering to the surface. However, the end portion of the steel sheet often turns yellow when the low-speed sheet passing area or at the end of the continuous sheet passing line at the end of the continuous sheet passing line, which is a problem in product quality. These yellow discolorations are a kind of rust, and the steel strip whose scale has been removed by pickling is generated by the combination of water and oxygen in the air, or it appears on the steel strip surface after pickling. The attached iron salt is generated by, for example, reacting with oxygen in the presence of sufficient water to produce ferric hydroxide.

【0003】従来、このようにして発生した黄変色の除
去方法もしくは発生の防止方法として次の方法がとられ
て来た。 (イ) 鉄塩を鋼帯表面に残存させないために、清浄なリン
ス水で十分に洗浄する。 (ロ) 低速通板時に鋼帯表面が乾燥して大気と接触して酸
化するのを防止するため、ドライヤーで瞬間乾燥させる
まで湿潤状態に保持する。 (ハ) 発生した黄変色をブラシや化学薬品等で連続して除
去するか、もしくは実開昭62−41072の如く酸洗
槽液をスプレーして除去する。 (ニ) 特開昭59−185786のように鋼板変色防止剤
を含有させたリンス液をスプレーして変色を抑制する。 等の方法が講じられてきた。
Conventionally, the following method has been employed as a method for removing or preventing the occurrence of yellow discoloration thus generated. (B) Wash thoroughly with clean rinsing water to prevent iron salts from remaining on the steel strip surface. (B) In order to prevent the surface of the steel strip from drying and being oxidized by contact with the atmosphere during low-speed passing, the steel strip is kept moist until it is instantaneously dried by a dryer. (C) The generated yellow discoloration is continuously removed with a brush, a chemical, or the like, or is removed by spraying a pickling bath solution as shown in Japanese Utility Model Laid-Open No. 62-41072. (D) Discoloration is suppressed by spraying a rinsing liquid containing a steel sheet discoloration inhibitor as disclosed in JP-A-59-185786. And so on.

【0004】[0004]

【発明が解決しようとする課題】これらの従来技術で
は、発生した黄変色が強度の場合は、これを除去するこ
とが困難であり、また、ブラシ等で除去する対策も、鋼
板表面にスクラッチ模様が残り、商品価値を著しく低下
する等の欠点を有している。本発明の目的は鋼帯の連続
酸洗の最終段階で発生する鋼板表面上の錆もしくは黄変
色を簡単な方法で解決し、錆もしくは黄変色を除去して
定常部と同様の鋼帯表面品質を保証できる連続酸洗付加
方法を提供するにある。
In these prior arts, if the generated yellow discoloration is intense, it is difficult to remove it, and a measure for removing it with a brush or the like is not enough. However, there is a disadvantage that the commercial value is significantly reduced. An object of the present invention is to solve rust or yellow discoloration on the steel sheet surface generated in the final stage of continuous pickling of a steel strip by a simple method, remove rust or yellow discoloration, and remove the rust or yellow discoloration to obtain the same steel strip surface quality as a stationary part. It is an object of the present invention to provide a continuous pickling addition method which can guarantee the pickling.

【0005】本発明の要旨とするところは次の如くであ
る。すなわち、連続的に鋼帯を酸洗するラインにおける
低速通板域もしくは通板停止時に発生する鋼表面上の
錆もしくは黄変色を除去する連続酸洗付加方法におい
て、前記鋼の通板方向を逆転して前記錆または黄変色
部を再度酸洗槽に浸漬した後、該逆転通板材付着した
酸液を酸洗槽入側において除去し、しかる後、再度正転
し前記錆または黄変色部を酸洗除去することを特徴とす
る鋼帯の連続酸洗付加方法、である。
The gist of the present invention is as follows. That is, in the continuous pickling addition method for removing rust or yellow discoloration on the steel strip surface generated at the time of a low-speed passing area or when the passing of the steel strip is stopped in a line for continuously pickling the steel strip , Reverse the rust or yellow discoloration
After the part is immersed again in the pickling tank, the acid solution attached to the reverse passing plate material is removed at the pickling tank entrance side, and then , the normal rotation is again performed to pickle and remove the rust or yellow discolored part. The method is a continuous pickling addition method for a steel strip.

【0006】本発明の実施例を添付図面を参照して説明
する。図1において、熱間圧延を終了した鋼帯2は、そ
の表面に付着した酸化鉄を除去するために、連続酸洗ラ
インの酸洗槽4に浸漬され、図において左から右方向へ
進行し、酸洗槽出側リンガーロール7にて酸液を絞り取
られ、複数個のリンススプレー8によって清浄水をスプ
レーされリンスされた後、再びリンス出側リンガーロー
ル11にて付着清浄水を絞り取られた後、ドライヤー1
2にて瞬間乾燥されて成品となる。ところが、これらの
酸洗工程を経た鋼帯に往々にして錆もしくは黄変色が発
生し、成品の商品価値を低下することがある。本発明は
この黄変色を除去するため次の酸洗付加方法をとる。
An embodiment of the present invention will be described with reference to the accompanying drawings. In FIG. 1, the steel strip 2 after hot rolling is immersed in a pickling tank 4 of a continuous pickling line in order to remove iron oxide adhering to its surface, and proceeds from left to right in the figure. After the acid solution is squeezed out by the ringer roll 7 on the pickling tank outlet side, the clean water is sprayed by a plurality of rinsing sprays 8 and rinsed, and the adhered clean water is squeezed again by the ringer roll 11 on the rinsing outlet side. After the dryer 1
It is dried instantly in 2 and becomes a product. However, rust or yellow discoloration often occurs in the steel strip that has undergone these pickling steps, which may lower the commercial value of the product. In the present invention, the following pickling addition method is employed to remove this yellow discoloration.

【0007】上記の如く、酸洗末期の鋼帯の低速通板域
もしくは通板停止時に黄変色部を発生した場合には、鋼
帯2の進行を逆転して再度、黄変色部を酸洗槽4に浸漬
する。かくして黄変色部を有する鋼帯2は、逆進行して
図において右から左方向へ進み、黄変色部が酸洗されて
消滅する。逆進行時、鋼帯表面に付着した酸液5は酸洗
槽4の入側において酸洗槽入側リンガーロール6によっ
て絞りとられ、新たに設けたスプレーロール14によっ
て完全に洗浄される。鋼帯の逆転による黄変色部の除去
が完了すると鋼帯は再び正転方向に巻き取られ、黄変色
部が除去された良好な製品を得ることができる。
[0007] As described above, when a yellow discolored portion occurs at the low speed passing area of the steel strip at the end of pickling or when the sheet is stopped, the progress of the steel strip 2 is reversed and the yellow discolored part is pickled again. Immerse in tank 4. Thus the steel strip 2 with a yellow discoloration proceeds in Figure from right to reverse traveling to the left, yellow discoloration disappears been pickled. During reverse movement, the acid solution 5 adhering to the steel strip surface is pickled.
At the entry side of the tank 4, it is squeezed by the ringer roll 6 on the entry side of the pickling tank, and is completely washed by the newly provided spray roll 14. When the removal of the yellow discolored portion due to the reverse rotation of the steel strip is completed, the steel strip is wound again in the normal direction, and a good product from which the yellow discolored portion has been removed can be obtained.

【0008】熱間圧延後の鋼帯の酸洗末期の低速通板域
もしくは通板停止時に発生した黄変色部の処理について
は従来、多くの方法が採られていたが、いずれも十分な
対策とはなっていなかったのに鑑み、本発明は、鋼帯を
逆転して黄変色部を再度酸洗する方法をとることにした
ので、次の効果を得ることができた。 (イ)黄変色部が定常部と同等の品質を確保することが
できた。 (ロ)逆転、再度の酸洗という簡単な酸洗付加方法によ
って、定常部と同一の品質を保証できるが、この付加作
業を遂行するにリンススプレー装置、ドライヤー等僅か
な設備増加で可能となり、作業も至極簡単で終了する。
Conventionally, many methods have been adopted for the treatment of the yellow discolored portion generated at the end of the pickling of a steel strip after hot rolling in the low-speed passing area or at the time of stopping the passing of the steel strip. In view of the above, the present invention has adopted the method of reversing the steel strip and pickling the yellow discolored portion again, so that the following effects can be obtained. (A) The quality of the yellow discolored portion was equal to that of the steady portion. (B) The same quality as the stationary part can be assured by a simple pickling addition method of reversing and pickling again. However, this additional work can be performed with a slight increase in equipment such as a rinsing sprayer and dryer. The work is extremely easy and ends.

【図面の簡単な説明】[Brief description of the drawings]

【図1】鋼帯の酸洗設備ならびに本発明による酸洗付加
方法を説明する酸洗装置を示す模式断面図である。
FIG. 1 is a schematic sectional view showing a pickling equipment for a steel strip and a pickling apparatus for explaining a pickling addition method according to the present invention.

【符号の説明】[Explanation of symbols]

2 鋼帯 4 酸洗槽 6 酸洗槽入側リンガーロール 7 酸洗槽出側リンガーロール 8 リンススプレー 10 リンガーロール 11 リンガーロール(リンス出側) 12 ドライヤー 14 新設リンススプレー 2 Steel strip 4 Pickling tank 6 Ringer roll on pickling tank inlet 7 Ringer roll on pickling tank outlet 8 Rinse spray 10 Ringer roll 11 Ringer roll (rinse outlet side) 12 Dryer 14 New rinse spray

Claims (1)

(57)【特許請求の範囲】(57) [Claims] 【請求項1】 連続的に鋼帯を酸洗するラインにおける
低速通板域もしくは通板停止時に発生する鋼表面上の
錆もしくは黄変色を除去する連続酸洗付加方法におい
て、前記鋼の通板方向を逆転して前記錆または黄変色
部を再度酸洗槽に浸漬した後、該逆転通板材付着した
酸液を酸洗槽入側において除去し、しかる後、再度正転
し前記錆または黄変色部を酸洗除去することを特徴とす
る鋼帯の連続酸洗付加方法。
1. A continuous continuous pickling additional process for removing rust or yellowing on the steel strip surface which is generated when stopping the low-speed communication leaf area or passing plate in line for pickling a steel strip, the steel strip Reverse the passing direction to rust or discolor yellow
After the part is immersed again in the pickling tank, the acid solution attached to the reverse passing plate material is removed at the pickling tank entrance side, and then , the normal rotation is again performed to pickle and remove the rust or yellow discolored part. Characteristic method of continuous pickling of steel strip.
JP3263140A 1991-09-13 1991-09-13 Continuous pickling method for steel strip Expired - Fee Related JP3048704B2 (en)