JP2945648B2 - Decorative painted metal sheet and method for producing the same - Google Patents

Decorative painted metal sheet and method for producing the same

Info

Publication number
JP2945648B2
JP2945648B2 JP3177598A JP3177598A JP2945648B2 JP 2945648 B2 JP2945648 B2 JP 2945648B2 JP 3177598 A JP3177598 A JP 3177598A JP 3177598 A JP3177598 A JP 3177598A JP 2945648 B2 JP2945648 B2 JP 2945648B2
Authority
JP
Japan
Prior art keywords
cross
linking
glossiness
metal sheet
crosslinking
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP3177598A
Other languages
Japanese (ja)
Other versions
JPH11227097A (en
Inventor
岳史 渡瀬
博昭 中野
敦史 木原
忠繁 中元
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Kobe Steel Ltd
Original Assignee
Kobe Steel Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Kobe Steel Ltd filed Critical Kobe Steel Ltd
Priority to JP3177598A priority Critical patent/JP2945648B2/en
Publication of JPH11227097A publication Critical patent/JPH11227097A/en
Application granted granted Critical
Publication of JP2945648B2 publication Critical patent/JP2945648B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Description

【発明の詳細な説明】DETAILED DESCRIPTION OF THE INVENTION

【0001】[0001]

【発明の属する技術分野】本発明は、家庭電気製品等に
繁用される意匠性塗装金属板(プレコート鋼板)に関
し、詳細には、如何なる受光角においても光沢度の最大
値が10以下の低光沢を有する所謂ちぢみ模様が付与さ
れた意匠性塗装金属板定に関するものである。本発明の
金属板は、アルミニウム板や銅板の他、冷延鋼板、溶融
亜鉛めっき鋼板、電気亜鉛めっき鋼板、合金化溶融亜鉛
めっき鋼板、ステンレス鋼板、銅めっき鋼板、錫めっき
鋼板等の種々の鋼板に適用される。尚、以下の記載では
その代表例として鋼板を中心に説明するが、決してこれ
に限定する趣旨ではない。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a design-coated metal plate (pre-coated steel plate) commonly used in household electric appliances and the like, and more particularly, to a low gloss having a maximum value of 10 or less at any light receiving angle. The present invention relates to a decorative painted metal plate provided with a so-called fine pattern having gloss. The metal sheet of the present invention is not limited to aluminum sheets and copper sheets, and various steel sheets such as cold-rolled steel sheets, hot-dip galvanized steel sheets, electro-galvanized steel sheets, galvannealed steel sheets, stainless steel sheets, copper-plated steel sheets, tin-plated steel sheets, and the like. Applied to In the following description, a steel sheet will be mainly described as a typical example, but the present invention is not limited to this.

【0002】[0002]

【従来の技術】従来より家庭電気製品用として、亜鉛系
めっき鋼板にスプレー塗装,電着塗装,粉体塗装等が施
された塗装鋼板が広く用いられてきた。しかし、近年で
は家電メーカーにおける塗装工程の省略を目的としたプ
レコート鋼板が繁用される様になっている。
2. Description of the Related Art A coated steel sheet obtained by applying a spray coating, an electrodeposition coating, a powder coating or the like to a zinc-coated steel sheet has been widely used for household electric appliances. However, in recent years, pre-coated steel sheets for the purpose of omitting the painting process in home appliance manufacturers have become popular.

【0003】ところでVTRやオーディオ等の家電製品
では、深みや落ち着き感のあるプレコート鋼板が求めら
れており、この様な要求特性を満足させるべく、光沢度
の低い低光沢鋼板が提案されている。一般に塗膜の光沢
を低下させる方法としては、塗料中の顔料濃度を増加し
たり、ビーズ等の充填剤を添加したり、更には無水ケイ
酸質の微粉末等の艶消し剤を添加する等の方法が採用さ
れている。
[0003] For home electric appliances such as VTRs and audios, pre-coated steel sheets having a sense of depth and calm have been demanded, and low gloss steel sheets having low gloss have been proposed in order to satisfy such required characteristics. In general, methods for reducing the gloss of the coating film include increasing the pigment concentration in the paint, adding a filler such as beads, and further adding a matting agent such as silicic acid fine powder. The method is adopted.

【0004】例えば特開昭63−158246には、被
膜形成成分に、種々の無機粉末及び硬化樹脂粉末を所定
量添加した低光沢塗装鋼板が開示されている。この方法
によれば、或る角度での光沢度は低くすることはできる
が、角度を種々変化させると光沢度が大きく変化し、見
る角度によっては光沢度が大きくなってしまう為、これ
では所望の要求特性に充分応えたものとは言えない。
For example, Japanese Patent Application Laid-Open No. 63-158246 discloses a low gloss coated steel sheet in which various inorganic powders and hardened resin powders are added in predetermined amounts to a film forming component. According to this method, the glossiness at a certain angle can be lowered, but if the angle is changed variously, the glossiness changes greatly, and the glossiness increases depending on the viewing angle. However, it cannot be said that the required characteristics have been sufficiently satisfied.

【0005】[0005]

【発明が解決しようとする課題】本発明は、上記事情に
着目してなされたものであり、その目的は、角度を種々
変化させた場合であっても光沢度のバラツキが小さく且
つ低光沢(光沢度の最大値が10以下)を満足する、所
謂ちぢみ模様の付与された意匠性塗装金属板、およびこ
の様な金属板を効率よく製造することのできる方法を提
供することにある。
SUMMARY OF THE INVENTION The present invention has been made in view of the above circumstances, and has as its object to reduce the variation in gloss and reduce the gloss even when the angle is variously changed. It is an object of the present invention to provide a design-coated metal plate provided with a so-called fine pattern, which satisfies the maximum value of the glossiness of 10 or less), and a method capable of efficiently producing such a metal plate.

【0006】[0006]

【課題を解決するための手段】上記課題を達成すること
のできた本発明の意匠性塗装金属板は、60゜鏡面光沢
度の最大値が10以下であり、且つ下式(1)で求めら
れる標準偏差σが1.5以下であるところに要旨を有す
る。
The design-coated metal sheet of the present invention, which has achieved the above-mentioned objects, has a maximum value of 60 ° specular gloss of 10 or less and is obtained by the following equation (1). The point is that the standard deviation σ is 1.5 or less.

【0007】[0007]

【数2】 (Equation 2)

【0008】この様な要件を満足する本発明の塗装金属
板は、所謂ちぢみ模様が付与されたものである。
[0008] The coated metal plate of the present invention satisfying such requirements is provided with a so-called crepe pattern.

【0009】また、上記課題を解決し得た本発明の製造
方法とは、 架橋性発現温度が30℃以上異なる感熱型架橋剤を2
種使用する(焼付け温度は、使用した感熱型架橋剤の架
橋性発現温度のいずれよりも高くすることが好ましい)
か、或いは 揮発性ブロック剤でブロックされた架橋触媒を用いる
ところに要旨を有するものである。
Further, the production method of the present invention which can solve the above-mentioned problems is characterized in that a heat-sensitive cross-linking agent whose cross-linking expression temperature differs by 30 ° C. or more is used.
Seeds are used (the baking temperature is preferably higher than any of the cross-linking expression temperatures of the heat-sensitive cross-linking agent used).
Alternatively, the gist is that a cross-linking catalyst blocked with a volatile blocking agent is used.

【0010】[0010]

【発明の実施の形態】前述した様に、従来「低光沢塗装
鋼板」と呼ばれるものは全て、或る一定角度における光
沢度を低くしたものであり、角度を変化させた場合に光
沢度が変化し、大きくなってしまうことについて全く考
慮していない。即ち、一般に光沢度は、60゜鏡面光沢
度(入射角60゜,受光角60゜)で測定しており、当
該受光角度における光沢度が10以下のものは知られて
いるが、受光角を種々変化させると光沢度が変化し、受
光角により光沢度が大きく変化してしまう。従って、こ
れでは「深みや落ち着き感のある」鋼板が得られず、所
望の要求特性に充分応えたものとは言えない。
DESCRIPTION OF THE PREFERRED EMBODIMENTS As described above, all of the conventional "low-gloss coated steel sheets" have a reduced glossiness at a certain angle, and the glossiness changes when the angle is changed. No consideration is given to the fact that it will grow. That is, the glossiness is generally measured at 60 ° specular glossiness (incident angle 60 °, light receiving angle 60 °), and it is known that the glossiness at the light receiving angle is 10 or less. Various changes change the glossiness, and the glossiness greatly changes depending on the light receiving angle. Accordingly, a steel sheet having a “depth and calmness” cannot be obtained with this method, and it cannot be said that the steel sheet sufficiently satisfies desired required characteristics.

【0011】そこで本発明者らは、受光角を種々変化さ
せたとしても光沢度が小さく、且つそのバラツキも小さ
い塗装鋼板(所謂ちぢみ模様の付与された鋼板)を提供
すべく鋭意検討した結果、所定の感熱型架橋剤若しくは
架橋触媒を使用して鋼板を製造すれば、あらゆる角度で
光を散乱することができ、所期の目的が見事に達成され
ることを見出し、本発明を完成したのである。
The inventors of the present invention have conducted intensive studies to provide a coated steel sheet (a steel sheet provided with a so-called crumpled pattern) having a small gloss and a small variation even when the light receiving angle is variously changed. If a steel sheet is manufactured using a predetermined heat-sensitive crosslinking agent or a crosslinking catalyst, light can be scattered at any angle, and it has been found that the intended purpose is achieved brilliantly. is there.

【0012】即ち、本発明の意匠性塗装金属板は、60
゜の入射角に対して測定される光沢度の最大値が10以
下であり、且つ上式(1)で求められる標準偏差σが
1.5以下を満足するものである。
That is, the decorative coated metal plate of the present invention has a size of 60
The maximum value of the glossiness measured with respect to the incident angle of ゜ is 10 or less, and the standard deviation σ obtained by the above equation (1) satisfies 1.5 or less.

【0013】詳細には、日本電色製光沢度計VGS−Σ
90を用い、図1に示す方法で光沢度を測定したときの
60゜鏡面光沢度の最大値が10以下であり、且つ上式
(1)で求められる標準偏差σが1.5以下を満足する
ものである。このことは、入射角を60゜とし、受光角
を50〜75゜の範囲で種々変化させて5゜間隔で光沢
度を測定した場合、光沢度が最も大きくなったとしても
10以下と小さく、且つ、当該受光角の範囲における光
沢度の標準偏差も1.5以下とバラツキが低く抑えられ
ることを意味する。
More specifically, a gloss meter VGS-II manufactured by Nippon Denshoku Co., Ltd.
When the glossiness is measured by the method shown in FIG. 1 using 90, the maximum value of 60 ° specular glossiness is 10 or less, and the standard deviation σ obtained by the above equation (1) satisfies 1.5 or less. Is what you do. This means that when the incident angle is set to 60 ° and the light receiving angle is variously changed in the range of 50 to 75 ° and the glossiness is measured at 5 ° intervals, the glossiness is as small as 10 or less even if the glossiness is maximized. In addition, the standard deviation of the glossiness in the range of the light receiving angle is 1.5 or less, which means that the variation can be suppressed low.

【0014】このことを明確にする為、図2に後記する
実施例の一部をグラフ化して示す。図2は、受光角を0
〜75゜の範囲で変化させた場合における各受光角の光
沢度をプロットしたものである。本発明例も従来例も受
光角0〜50゜付近までは同様の挙動を示すが、50゜
付近を超えると両者の違いは明瞭になる。即ち、本発明
例(図中○,△)では、いずれも光沢度の最大値が10
以下(受光角60゜付近)であり、且つ上式(1)で表
される標準偏差σも1.5以下と小さいのに対し、従来
例(図中□)では、60゜付近になると光沢度が非常に
高くなり、最大値が10を超えてしまう。また、他の従
来例(図中◇)では、光沢度の最大値は10以下に抑え
られるものの、受光角60゜近傍(60゜±10゜前
後)では光沢度が大きく変化し、光沢度のバラツキが極
めて大きくなる。次に、この様な本発明金属板を製造す
る方法について説明する。
To clarify this, FIG. 2 is a graph showing a part of the embodiment described later. FIG.
7 is a plot of the glossiness at each light receiving angle when changed in the range of up to 75 °. Both the present invention example and the conventional example show the same behavior up to a light receiving angle of around 0 ° to 50 °, but the difference between them becomes clear above 50 °. That is, in the examples of the present invention (○ and Δ in the figure), the maximum value of the gloss was 10
(The light receiving angle is around 60 °), and the standard deviation σ represented by the above equation (1) is as small as 1.5 or less, whereas in the conventional example (□ in the figure), the gloss becomes near 60 °. The degree becomes very high and the maximum value exceeds 10. Further, in another conventional example ((in the figure), the maximum value of the glossiness is suppressed to 10 or less, but the glossiness changes greatly near the light receiving angle of 60 ° (around 60 ° ± 10 °), and the glossiness changes. The variation becomes extremely large. Next, a method for manufacturing such a metal plate of the present invention will be described.

【0015】本発明は、上述した様にあらゆる角度で光
を散乱し得る所謂ちぢみ模様が付与されたものである
が、基本的には、塗膜内部が硬化する前に塗膜表面を硬
化させることによって得られる。即ち、塗膜表面と内部
の硬化速度に差を設けることにより、任意のちぢみ模様
を付与しようというものであり、硬化初期には表層が硬
化収縮し、硬化の後期には下層の収縮歪みを表層が吸収
することにより、表面にちぢみが付与されるのである。
Although the present invention is provided with a so-called crepe pattern which can scatter light at any angle as described above, basically, the surface of the coating film is cured before the inside of the coating film is cured. Obtained by: That is, by providing a difference in the curing speed between the coating film surface and the inside, it is intended to impart an arbitrary fine pattern, the surface layer cures and contracts in the early stage of curing, and the contraction distortion of the lower layer in the later stage of curing causes the surface layer to contract. The absorption of the particles gives the surface a blemishes.

【0016】この様に本発明法は、所定のちぢみ模様が
得られる様、塗膜中に所定の添加剤を添加したところに
最重要ポイントがあるが、具体的には、下記または
の添加剤を使用することができる。
As described above, according to the method of the present invention, the most important point is that a predetermined additive is added to a coating film so that a predetermined shrinkage pattern can be obtained. Can be used.

【0017】架橋性発現温度が30℃以上異なる2種
の感熱型架橋剤を使用する方法 上記感熱型架橋剤は、架橋成分(イソシアネート類)と
ブロック剤(アルコール類、フェノール類、ε−カプロ
ラクタム等)とからなるものである。この架橋剤は、ブ
ロック化している状態では不活性であるが、熱風炉等に
より加熱するとブロック剤が解離し、架橋成分が活性化
してベース樹脂と架橋反応を起こす様になる。塗膜中
に、架橋性発現温度の異なる2種類の感熱型架橋剤[低
温解離型架橋剤(架橋性発現温度Ta)と高温解離型架
橋剤(架橋性発現温度Tb)]を添加しておけば、加熱
によって、まず、低温解離型架橋剤が塗膜表面に移動
し、このうちのブロック剤が解離して架橋成分が活性化
することにより所謂ちぢみ模様が形成される様になる。
Method of using two types of heat-sensitive cross-linking agents whose cross-linking expression temperatures differ by 30 ° C. or more The heat-sensitive cross-linking agent comprises a cross-linking component (isocyanates) and a blocking agent (alcohols, phenols, ε-caprolactam, etc.). ). This cross-linking agent is inactive in a blocked state, but when heated by a hot air oven or the like, the blocking agent is dissociated, and the cross-linking component is activated to cause a cross-linking reaction with the base resin. Two kinds of heat-sensitive cross-linking agents having different cross-linking temperature (cross-linking temperature (Tb) and high-temperature dissociating cross-linking agent (cross-linking temperature Ta)) can be added to the coating film. For example, by heating, first, the low-temperature dissociation type cross-linking agent moves to the coating film surface, and the blocking agent among them dissociates to activate the cross-linking component, thereby forming a so-called shrinking pattern.

【0018】尚、架橋性発現温度は使用するブロック剤
の種類によって変化させることができるが、ちぢみ模様
を付与するには、その温度差を30℃以上(Tb−Ta
≧30℃)にすることが必要である。尚、この温度差は
大きければ大きい程好ましいが、大きくなり過ぎると所
謂ワキと呼ばれる塗装欠陥(塗膜表層に被膜が形成され
ている状態で、塗料中の溶剤が揮発する際に発生する欠
陥)が発生し易くなること等を考慮すれば、60℃以下
にすることが推奨される。
The temperature at which the crosslinking property is exhibited can be varied depending on the type of the blocking agent used. To provide a shrink pattern, the temperature difference must be 30 ° C. or more (Tb-Ta).
≧ 30 ° C.). The temperature difference is preferably as large as possible. However, if the temperature difference is too large, so-called coating defects (defects generated when the solvent in the coating material evaporates in a state where the coating is formed on the surface of the coating film). Considering that the occurrence of cracks easily occurs, it is recommended that the temperature be 60 ° C. or lower.

【0019】塗膜中に占める上記低温解離型架橋剤と高
温解離型架橋剤の含有量は合計で、樹脂100重量部に
対し、3〜30重量部とすることが好ましい。含有量が
30重量部を超えると塗膜の架橋密度が上昇し、塗膜の
伸びが低下する為、塗膜形成後に加工を必要とするプレ
コート金属板にとって好ましくない。より好ましくは2
0重量部以下である。一方、含有量が3重量部未満にな
ると、架橋剤による添加効果が小さく、所望のちぢみ効
果が得られない。より好ましくは5重量部以上である。
尚、これらの比率は、低温解離型架橋剤:高温解離型架
橋剤=3〜7:7〜3とすることが推奨される。
The total content of the low-temperature dissociative crosslinking agent and the high-temperature dissociative crosslinking agent in the coating film is preferably 3 to 30 parts by weight based on 100 parts by weight of the resin. If the content exceeds 30 parts by weight, the crosslink density of the coating film increases, and the elongation of the coating film decreases, which is not preferable for a precoated metal sheet that requires processing after forming the coating film. More preferably 2
0 parts by weight or less. On the other hand, if the content is less than 3 parts by weight, the effect of the addition by the crosslinking agent is small, and the desired shrinking effect cannot be obtained. It is more preferably at least 5 parts by weight.
In addition, it is recommended that these ratios are set as low-temperature dissociation type crosslinking agent: high-temperature dissociation type crosslinking agent = 3-7: 7-3.

【0020】また、焼付け温度は、高温解離型架橋剤の
架橋性発現温度(Tb)よりも高くすることが好まし
く、これにより、所望のちぢみ模様を効率よく得ること
ができる。より好ましくは10℃以上高くすることが推
奨される。
The baking temperature is preferably higher than the cross-linking temperature (Tb) of the high-temperature dissociation type cross-linking agent, whereby a desired shrink pattern can be efficiently obtained. More preferably, it is recommended to raise the temperature by 10 ° C. or more.

【0021】揮発性ブロック剤でブロックされた架橋
触媒を用いる方法 上記架橋触媒は、揮発性ブロック剤(アミン)と触媒成
分(スルホン酸)からなるものである。この架橋触媒
は、ブロック化している状態では不活性であるが、熱風
炉等により加熱するとブロック剤が解離し、揮発したブ
ロック剤は熱風により系外に排出される一方、活性化し
た触媒成分は、ベース樹脂と架橋剤の架橋反応を促進
し、結果的にちぢみ模様が付与されることになる。
Method Using a Crosslinking Catalyst Blocked with a Volatile Blocking Agent The above crosslinking catalyst comprises a volatile blocking agent (amine) and a catalyst component (sulfonic acid). This cross-linking catalyst is inactive when it is blocked, but when heated by a hot air oven or the like, the blocking agent is dissociated, and the volatilized blocking agent is discharged out of the system by hot air, while the activated catalyst component is The cross-linking reaction between the base resin and the cross-linking agent is promoted, and consequently, a shrinking pattern is provided.

【0022】上記架橋触媒は、塗膜中の樹脂100重量
部につき、0.1〜1.5重量部添加することが好まし
い。1.5重量部を超えると多量の触媒の添加により、
塗膜表層のみならず内層部でも架橋する為、所望のちぢ
み外観が得られない。一方、0.1重量部未満では、触
媒の効果が不充分であり、やはり所望のちぢみ外観が得
られない。
The crosslinking catalyst is preferably added in an amount of 0.1 to 1.5 parts by weight per 100 parts by weight of the resin in the coating film. If it exceeds 1.5 parts by weight, a large amount of catalyst is added,
Crosslinking occurs not only in the surface layer of the coating film but also in the inner layer portion, so that a desired fine appearance cannot be obtained. On the other hand, if it is less than 0.1 part by weight, the effect of the catalyst is insufficient, and the desired fine appearance cannot be obtained.

【0023】また、上記方法に用いられる架橋剤として
は通常のプレコート鋼板に使用されるものであれば特に
限定されず、例えばメラミン系樹脂等が挙げられる。
The cross-linking agent used in the above method is not particularly limited as long as it is used for ordinary precoated steel sheets, and examples thereof include melamine resins.

【0024】この様に本発明法は、塗膜中に上記又は
の添加剤を必須的に含有するものであるが、更に本発
明の作用を損なわない範囲でワックス、骨材、顔料、消
泡剤、レベリング剤、アルミ等の金属片等を添加するこ
とができる。
As described above, according to the method of the present invention, the above-mentioned or the above-mentioned additives are essentially contained in the coating film, but the wax, aggregate, pigment, defoamer and the like can be used as long as the action of the present invention is not impaired. Agents, leveling agents, metal pieces such as aluminum and the like can be added.

【0025】また、本発明における塗膜に使用される塗
料樹脂は、要するに架橋剤を使用し得るものであれば特
に限定されず、エポキシ系、ポリエステル系、アクリル
系、メラミン系、ウレタン系、シリコン系等の溶剤希釈
型塗料;アクリル−スチレン系、エポキシ−エステル
系、アクリル系、ウレタン系、ポリ酢酸ビニル系、ポリ
エチレン系、エチレン酢酸ビニル系等の水系エマルジョ
ン系型塗料などが挙げられる。これらは単独で使用して
も良いし、2種以上を併用しても構わない。
The coating resin used in the coating film of the present invention is not particularly limited as long as it can use a crosslinking agent. Epoxy, polyester, acrylic, melamine, urethane, silicone and the like. Solvent-dilutable paints such as acrylic-styrene, epoxy-ester, acrylic, urethane, polyvinyl acetate, polyethylene, and ethylene vinyl acetate paints. These may be used alone or in combination of two or more.

【0026】本発明鋼板の製造に当たっては、上記又
はの添加剤を必須的に含む塗料を素地金属板に塗布
し、焼付けて塗膜を形成させれば良い。塗布に当たって
は、通常のプレコート金属板に使用される方法を採用す
ることができ、例えばロールコーター法、カーテンフロ
ー法等が挙げられる。
In producing the steel sheet of the present invention, a paint containing the above or the above-mentioned additives is applied to a base metal plate and baked to form a coating film. For application, a method used for a normal pre-coated metal plate can be adopted, and examples thereof include a roll coater method and a curtain flow method.

【0027】以下実施例に基づいて本発明を詳述する。
ただし、下記実施例は本発明を制限するものではなく、
前・後記の趣旨を逸脱しない範囲で変更実施することは
全て本発明の技術範囲に包含される。
Hereinafter, the present invention will be described in detail with reference to examples.
However, the following examples do not limit the present invention,
All modifications and alterations without departing from the spirit of the preceding and following descriptions are included in the technical scope of the present invention.

【0028】[0028]

【実施例】実施例1 プライマー塗装したクロメート処理亜鉛めっき鋼板に、
表1及び2に示す種々の塗料成分(A〜J)をロールコ
ーターで塗布し、塗膜の乾燥重量が30g/m 2 となる
様にした。その後、熱風炉にて到達温度230℃で60
秒間焼付けすることにより各供試材を得た。尚、上記塗
料成分A〜Jは、いずれもベース樹脂としてポリエステ
ル系樹脂を使用している。
Example 1 A chromate-treated galvanized steel sheet coated with a primer
Various paint components (A to J) shown in Tables 1 and 2 were
The dry weight of the coating film is 30 g / m Two Becomes
I did it. After that, at a temperature of 230 ° C in a hot air oven, 60
Each sample was obtained by baking for 2 seconds. The above coating
The ingredients A to J are all polyester resins as base resins.
The resin is used.

【0029】この様にして得られた各供試材における6
0゜鏡面光沢度を前記の方法により測定し、σで表され
る光沢度の標準偏差を算出すると共に、意匠性につき下
記方法で評価した。
In each of the thus obtained test materials, 6
The 0 ° specular gloss was measured by the above method, the standard deviation of the gloss represented by σ was calculated, and the design was evaluated by the following method.

【0030】[意匠性評価法]供試材の外観を目視で観
察し、下記基準にて評価した。 ○:あらゆる角度から見ても艶のない外観(艶消し外
観)が得られている。 △:特定の角度から見ると艶が目立ち、艶消し外観が得
られない。 ×:艶が非常に目立ち、艶消し外観でない。 これらの結果を表1及び2に併記する。
[Design Evaluation Method] The appearance of the test material was visually observed and evaluated according to the following criteria. :: A matte appearance (matte appearance) is obtained even from all angles. Δ: The gloss is conspicuous when viewed from a specific angle, and a matte appearance cannot be obtained. ×: The gloss is very conspicuous, and the appearance is not matte. The results are shown in Tables 1 and 2.

【0031】[0031]

【表1】 [Table 1]

【0032】[0032]

【表2】 [Table 2]

【0033】表より以下の様に考察することができる。
まず、A及びBは架橋性発現温度の異なる2種類の感熱
型架橋剤を使用した本発明例であるが、60゜での光沢
度(G60)10以下、σ1.5以下を満足し、且つ意匠
性にも優れている。
The following can be considered from the table.
First, A and B are examples of the present invention using two types of heat-sensitive crosslinking agents having different cross-linking development temperatures, and satisfy a gloss (G 60 ) at 60 ° of 10 or less and a σ of 1.5 or less. And it has excellent design.

【0034】これに対して、Cは低温解離型架橋剤のみ
を、Dは高温解離型架橋剤のみを使用した例であるが、
60が55若しくはそれ以上と高く、σも大きくなり、
特定の角度から見ると艶が目立ち、意匠性に劣る。
On the other hand, C is an example using only a low-temperature dissociation type crosslinking agent, and D is an example using only a high-temperature dissociation type crosslinking agent.
G 60 is as high as 55 or more, σ also increases,
When viewed from a specific angle, the gloss is conspicuous and the design is inferior.

【0035】次に、E〜Gは架橋剤と架橋触媒を両方使
用した本発明例であり、Fは更にビーズも添加したもの
であるが、いずれの場合においても、G6010以下、σ
1.5以下を満足し、意匠性にも優れている。
[0035] Then, E to G is the invention example using both the crosslinking agent crosslinking catalyst, F is but one in which further also added beads, in any case, G 60 10 or less, sigma
It satisfies 1.5 or less and has excellent design.

【0036】これに対してI及びJは架橋剤とビーズの
みを添加して架橋触媒を添加しない従来例、Hは架橋剤
のみを添加した従来例であるが、いずれもG60、σが大
きくなり、意匠性にも劣る。この傾向は特に、Hにおい
て顕著に見られた。
The conventional hand I and J without adding a crosslinking catalyst is added only crosslinking agent and beads, H but is a conventional example of adding only the cross-linking agent, both G 60, sigma is large Inferior in design. This tendency was particularly remarkable in H.

【0037】実施例2 次に、塗料成分Aについて、架橋性発現温度を種々変化
させた2種類の感熱型架橋剤を用い、意匠性について同
様に評価した。得られた結果を表3に示す。
Example 2 Next, with respect to the coating material component A, the design property was similarly evaluated using two types of heat-sensitive crosslinking agents having variously changed crosslinking developing temperatures. Table 3 shows the obtained results.

【0038】[0038]

【表3】 [Table 3]

【0039】No.1〜3は、架橋性発現温度が30℃以
上異なる感熱型架橋剤を使用した本発明例であるが、意
匠性に優れている。これに対し、架橋性発現温度が上記
要件を満足しないNo.4,5は意匠性に劣る。
Nos. 1 to 3 are examples of the present invention in which heat-sensitive cross-linking agents differing in cross-linking temperature by 30 ° C. or more are used, but are excellent in design. On the other hand, Nos. 4 and 5 whose cross-linking temperature does not satisfy the above requirements are inferior in design.

【0040】[0040]

【発明の効果】本発明の意匠性塗装金属板は上記の様に
構成されているので、受光角を種々変化させても光沢度
が小さく、且つそのバラツキも小さい所謂ちぢみ模様の
付与された金属板を効率よく得ることができた。
Since the decorative coated metal plate of the present invention is constructed as described above, even if the light receiving angle is changed variously, the glossiness is small, and the variation in the gloss is small. The board was obtained efficiently.

【図面の簡単な説明】[Brief description of the drawings]

【図1】入射角60゜における光沢度の測定方法を示す
説明図。
FIG. 1 is an explanatory diagram showing a method for measuring glossiness at an incident angle of 60 °.

【図2】実施例1の結果を示すグラフ。FIG. 2 is a graph showing the results of Example 1.

───────────────────────────────────────────────────── フロントページの続き (72)発明者 中元 忠繁 兵庫県加古川市金沢町1番地 株式会社 神戸製鋼所 加古川製鉄所内 (56)参考文献 特開 平6−316772(JP,A) 特開 平6−278245(JP,A) 特開 平4−31037(JP,A) 特開 平9−71750(JP,A) 特表 平5−508434(JP,A) (58)調査した分野(Int.Cl.6,DB名) B32B 15/08 B05D 7/14 ────────────────────────────────────────────────── ─── Continuation of the front page (72) Inventor Tadashige Nakamoto 1 Kanazawacho, Kakogawa City, Hyogo Prefecture Kobe Steel, Ltd. Kakogawa Works (56) References JP-A-6-316772 (JP, A) JP JP-A-6-278245 (JP, A) JP-A-4-31037 (JP, A) JP-A-9-71750 (JP, A) Table of contents JP-A-5-508434 (JP, A) (58) Fields investigated (Int) .Cl. 6 , DB name) B32B 15/08 B05D 7/14

Claims (5)

(57)【特許請求の範囲】(57) [Claims] 【請求項1】 60゜鏡面光沢度の最大値が10以下で
あり、且つ下式(1)で求められる標準偏差σが1.5
以下であることを特徴とする意匠性塗装金属板。 【数1】
1. The maximum value of 60 ° specular gloss is 10 or less, and the standard deviation σ obtained by the following equation (1) is 1.5.
A design painted metal plate characterized by the following. (Equation 1)
【請求項2】 ちぢみ模様が付与されたものである請求
項1に記載の意匠性塗装金属板。
2. The design-coated metal sheet according to claim 1, wherein the metal sheet is provided with a fine pattern.
【請求項3】 架橋性発現温度が30℃以上異なる感熱
型架橋剤を2種使用することを特徴とする請求項1また
は2に記載の意匠性塗装金属板の製造方法。
3. The method for producing a design-coated metal sheet according to claim 1, wherein two kinds of heat-sensitive crosslinking agents having different crosslinking expression temperatures differing by 30 ° C. or more are used.
【請求項4】 焼付け温度を、使用した感熱型架橋剤の
架橋性発現温度のいずれよりも高くするものである請求
項3に記載の製造方法。
4. The production method according to claim 3, wherein the baking temperature is higher than any of the cross-linking expression temperatures of the heat-sensitive crosslinking agent used.
【請求項5】 揮発性ブロック剤でブロックされた架橋
触媒を用いることを特徴とする請求項1または2に記載
の意匠性塗装金属板の製造方法。
5. The method according to claim 1, wherein a crosslinking catalyst blocked with a volatile blocking agent is used.
JP3177598A 1998-02-13 1998-02-13 Decorative painted metal sheet and method for producing the same Expired - Fee Related JP2945648B2 (en)