JP2809803B2 - Leather-like sheet - Google Patents

Leather-like sheet

Info

Publication number
JP2809803B2
JP2809803B2 JP8540690A JP8540690A JP2809803B2 JP 2809803 B2 JP2809803 B2 JP 2809803B2 JP 8540690 A JP8540690 A JP 8540690A JP 8540690 A JP8540690 A JP 8540690A JP 2809803 B2 JP2809803 B2 JP 2809803B2
Authority
JP
Japan
Prior art keywords
leather
sheet
collagen
polymer
polyurethane
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP8540690A
Other languages
Japanese (ja)
Other versions
JPH03287878A (en
Inventor
勝洋 日置
一人 赤股
祐太郎 谷
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Kuraray Co Ltd
Original Assignee
Kuraray Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Kuraray Co Ltd filed Critical Kuraray Co Ltd
Priority to JP8540690A priority Critical patent/JP2809803B2/en
Publication of JPH03287878A publication Critical patent/JPH03287878A/en
Application granted granted Critical
Publication of JP2809803B2 publication Critical patent/JP2809803B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Description

【発明の詳細な説明】 <産業上の利用分野> 本発明は、手に触れた感触が天然皮革のような汗を好
い込むようなぬめり感のないサラッとした質感及び良好
な吸汗性を有し、天然皮革に類似した見た目の重厚感と
色の深みがあり、かつマット調で濃く見える、表面強さ
に優れた皮革様シートに関するものである。
DETAILED DESCRIPTION OF THE INVENTION <Industrial Application Field> The present invention has a smooth texture and a good sweat-absorbing property, in which the touch of the hand touches sweat like natural leather without sliminess. Further, the present invention relates to a leather-like sheet which has a solid appearance and color depth similar to that of natural leather, has a mat-like appearance, and is excellent in surface strength.

<従来の技術> 従来、マット調の皮革様シートとしては、表面に極細
繊維の立毛を形成し、サンドペーパーなどによりバフィ
ングして毛足を短く整毛したもの、ポリウレタンなどの
弾性重合体の微多孔質被覆層を形成し、表面のスキン層
を研削除去し微細気孔の一部を露出させたものなどが提
案されている。しかし、これらはいずれも天然皮革でい
うスエードに近い外観であり、徽目の細かいマット調の
外観とは程遠いものであった。
<Conventional technology> Conventionally, as a mat-like leather-like sheet, nap of fine fibers is formed on the surface, buffed with sandpaper or the like to shorten the hair, and elastic polymer such as polyurethane is used. There have been proposed ones in which a porous coating layer is formed, and a skin layer on the surface is removed by grinding to expose a part of fine pores. However, all of them had an appearance close to a suede of natural leather, far from a matte appearance with a fine embossment.

また、皮革様シートの被覆層へ天然皮革粉末やコラー
ゲンなどを混入して天然皮革類似の外観及び質感を再現
する試みも多数提案されている。例えば特公昭63−2364
4号公報、特公昭63−315677号公報等が挙げられる。こ
れらの皮革様シートは単に粒径の大きい皮革粉末やコラ
ーゲン粉末などを混入しているのみであり、その表面状
態はマット調とは程遠いものであった。
Also, many attempts have been made to reproduce natural leather-like appearance and texture by mixing natural leather powder, collagen, and the like into the coating layer of the leather-like sheet. For example, Japanese Patent Publication 63-2364
No. 4, JP-B-63-315677, and the like. These leather-like sheets were merely mixed with leather powder or collagen powder having a large particle size, and the surface condition was far from matte.

<発明が解決しようとする課題> 本発明は、手に触れた感触が天然皮革のような汗を吸
い込むようなぬめり感のないサラッとした質感及び良好
な吸汗性を有し、天然皮革に類似した見た目の重厚感と
色の深みがあり、かつ徽目の細かいマット調で濃く見え
る、表面強さに優れた皮革様シートを提供するものであ
る。
<Problems to be Solved by the Invention> The present invention is similar to natural leather because it has a smooth texture and a good sweat-absorbing property that the touch to the hand does not have the slimy feeling of sucking sweat like natural leather. The object is to provide a leather-like sheet which has a solid appearance and depth of color, and which looks dark with a fine matte tone and excellent surface strength.

<課題を解決するための手段> 本発明は、繊維集合体に弾性重合体を主体とした重合
体を含有した基体層と弾性重合体を主体とした重合体の
被覆層とからなる皮革様シートにおいて、該被覆層の表
面が非繊維状で平均粒径10μ以下かつ見掛け嵩密度0.1
〜0.3g/cm3のコラーゲン粉末とポリウレタンを主体とし
た重合体との混合物よりなり微細な凹凸を有することを
特徴とする皮革様シートである。
<Means for Solving the Problems> The present invention provides a leather-like sheet comprising a base layer containing a polymer mainly composed of an elastic polymer in a fiber aggregate and a coating layer of a polymer mainly composed of an elastic polymer. In, the surface of the coating layer is non-fibrous, the average particle size is 10μ or less and apparent bulk density 0.1
A leather-like sheet comprising a mixture of collagen powder of about 0.3 g / cm 3 and a polymer mainly composed of polyurethane and having fine irregularities.

すなわち、本発明は、普通繊維、極細繊維および/ま
たはその束状繊維、特殊多孔繊維などのいずれかの繊維
で作られた織布、編布あるいは繊維絡合不織布などの繊
維集合体に、ポリウレタン、アクリル系重合体、アクリ
ロニトリル・ブタジエン共重合体、スチレン・ブタジエ
ン共重合体などの合成ゴムなどの弾性重合体の群から選
ばれた少なくとも1種類の弾性重合体を主体とした重合
体を含有させて得た、弾性重合体を主体とした重合体と
繊維集合体とからなる基体層、その基体層の一面にポリ
ウレタン、可塑化ポリ塩化ビニルなど弾性重合体を主体
とした重合体の多孔質層または非多孔質層を表面層とし
たシート状物を形成し、その表面にコラーゲン粉末を含
有したポリウレタン組成物液を塗布・乾燥して皮革様シ
ートを製造するものである。
That is, the present invention relates to a method of manufacturing a fiber assembly such as a woven fabric, a knitted fabric, or a fiber entangled nonwoven fabric made of any fiber such as ordinary fiber, ultrafine fiber and / or bundled fiber thereof, and special porous fiber. Containing an acrylic polymer, an acrylonitrile-butadiene copolymer, a polymer mainly composed of at least one elastic polymer selected from the group of elastic polymers such as synthetic rubbers such as a styrene-butadiene copolymer. Layer consisting of a polymer mainly composed of an elastic polymer and a fiber assembly obtained by the above method, and a porous layer of a polymer mainly composed of an elastic polymer such as polyurethane or plasticized polyvinyl chloride on one surface of the substrate layer. Alternatively, a sheet-like material having a non-porous layer as a surface layer is formed, and a polyurethane composition solution containing collagen powder is applied to the surface and dried to produce a leather-like sheet. A.

本発明の基体層は、通常の繊維、例えば、ポリエステ
ル、ポリアミド、ポリアクリロニトリル、ポリオレフイ
ン、ポリビニルアルコールなどの合成繊維、再生セルロ
ースなどの化学繊維、天然繊維、あるいは特殊形態の繊
維、例えば、ポリエステル、ポリアミド、ポリアクリロ
ニトリルなどの極細繊維あるいは少なくとも1成分を溶
解除去することにより極細繊維束状繊維や特殊多孔繊維
などに変成することのできる多成分繊維から選ばれた繊
維で構成されたニードルパンチや高速流体流により絡合
処理された繊維絡合不織布、繊維立毛編織布、不織布と
編織布の積層布などの布帛から選ばれた1種類の布帛
に、弾性重合体を主体とした含浸用組成液を含浸し、次
いで必要に応じ、一面に重合体の塗布用組成液を塗布し
て重合体の非溶剤中でスポンジ構造に凝固させ、多成分
繊維を極細繊維束状繊維や特殊多孔繊維に変成し、必要
に応じ更に弾性重合体を主体とした重合体被膜層を付与
したシート状物である。
The base layer of the present invention may be formed of ordinary fibers, for example, synthetic fibers such as polyester, polyamide, polyacrylonitrile, polyolefin, and polyvinyl alcohol, synthetic fibers such as regenerated cellulose, natural fibers, or fibers in a special form, for example, polyesters and polyamides. Needle punch or high-speed fluid composed of fibers selected from ultra-fine fibers such as polyacrylonitrile or multi-component fibers that can be transformed into ultra-fine fiber bundles or special porous fibers by dissolving and removing at least one component One type of fabric selected from a fabric entangled by flow, such as a fiber entangled nonwoven fabric, a fiber-woven knitted woven fabric, or a laminated fabric of a nonwoven fabric and a woven fabric, is impregnated with a composition liquid for impregnation mainly comprising an elastic polymer. Then, if necessary, then apply a polymer coating composition on one side and in a polymer non-solvent Solidifying the sponge structure, the multicomponent fibers and transformed into microfine fiber bundles fibers or special porous fibers, further elastic polymer sheet imparted with polymeric coating layer consisting mainly of needed.

基体層として通常の繊維、特にポリエステルやポリア
ミド繊維からなるものを使用すれば皮革様シートとした
とき適度の腰と保型性に優れたものとなり、極細繊維束
状繊維からなるものを使用すれば柔軟な風合いで靴に加
工したときトップラインがシャープに入り、また、特殊
多孔繊維からなるものを使用すれば適度の腰と軽量性を
合わせ持ったものとなり、表面のサラッとした質感や見
た目の重厚感、深みのある色調などと相俟って高級感に
溢れた人工皮革製品となる。
If the base layer is made of ordinary fibers, especially those made of polyester or polyamide fibers, the leather-like sheet becomes moderately stiff and excellent in shape retention, and if it is made of ultrafine fiber bundle fibers, When processed into shoes with a soft texture, the top line becomes sharp, and if you use special porous fiber, it will have a moderate waist and lightness, and the surface has a smooth texture and appearance It is an artificial leather product full of luxury, combined with a solid feeling and a deep color tone.

本発明で被覆層に使用するコラーゲンは、動物の皮
膚、骨、腱を酵素などにより処理精製し、高分子状のコ
ラーゲン繊維を抽出し、コラーゲン繊維間に架橋反応さ
せた後粉砕して得られる平均粒径2〜10μ、見掛け嵩密
度0.1〜0.3g/cm3であって、好ましくは最密充填嵩密度
0.4〜0.6g/cm3の非繊維状のコラーゲン粉末であり、例
えば昭和電工製のCX240やCX260などが挙げられる。該コ
ラーゲンの平均粒径が10μより大きいと表面にザラツキ
感が出て徽目の細かいスムースな面が得られず、天然皮
革様のスムースでナチュラルなタッチが得られない。ま
た、見掛密度が0.3g/cm3より大きくなると、コラーゲン
粒子の嵩高さが小さくなるため樹脂との親和性が低下し
塗膜強度が小さくなるとともに、徽目の細かいマット調
の外観とタッチが得られにくく耐久性も低下する。更
に、水分や汗を吸い込む能力が減少して目標とする吸汗
性が得られない。また、見掛け嵩密度が0.1g/cm3より小
さくなると、コラーゲン粒子の強度が小さくなり塗膜強
度が小さくなる。従って、樹脂との接着性を上げ徽目の
細かいマット調の仕上げ面を得るためにはコラーゲンの
平均粒径が10μ以下、見掛嵩密度が0.1〜0.3g/cm3の範
囲が好ましい。尚、本発明において見掛け嵩密度はJIS
K 6721により求めたものである。
The collagen used in the coating layer in the present invention is obtained by treating and purifying animal skin, bones and tendons with an enzyme or the like, extracting high molecular collagen fibers, causing a cross-linking reaction between the collagen fibers, and then pulverizing. the average particle diameter 2~10Myu, a apparent bulk density of 0.1 to 0.3 g / cm 3, preferably close-packed bulk density
A non-fibrous collagen powder of 0.4 to 0.6 g / cm 3 , such as CX240 or CX260 manufactured by Showa Denko. When the average particle size of the collagen is larger than 10 μm, the surface becomes rough and a fine smooth surface cannot be obtained, and a natural leather-like smooth and natural touch cannot be obtained. When the apparent density is greater than 0.3 g / cm 3 , the bulk of the collagen particles is reduced, so that the affinity with the resin is reduced, the coating strength is reduced, and the appearance and touch of the fine matte tone are reduced. Is difficult to obtain, and the durability also decreases. Furthermore, the ability to inhale moisture and sweat is reduced, and the desired sweat absorption property cannot be obtained. On the other hand, when the apparent bulk density is less than 0.1 g / cm 3 , the strength of the collagen particles decreases and the strength of the coating film decreases. Accordingly, in order to increase the adhesiveness to the resin and obtain a fine matte finish, it is preferable that the average particle size of collagen is 10 μm or less and the apparent bulk density is 0.1 to 0.3 g / cm 3 . In the present invention, the apparent bulk density is JIS
Determined by K 6721.

該コラーゲン粉末とポリウレタンを主体とした重合体
の重量比は1:1〜2:1の範囲である。コラーゲン粉末の量
が少なくなるとコラーゲンの特徴である吸汗性やサラッ
としたタッチが得られず、また、逆にコラーゲンの量が
多くなるとコラーゲン粉末が重合体により十分固定出来
ず、皮膜強度が低下するとともに風合いも悪くなる。
The weight ratio of the collagen powder to the polyurethane-based polymer is in the range of 1: 1 to 2: 1. If the amount of the collagen powder is small, the characteristic of collagen such as sweat absorption and a smooth touch cannot be obtained, and if the amount of collagen is large, the collagen powder cannot be sufficiently fixed by the polymer, and the film strength is reduced. The texture also worsens.

本発明で、コラーゲン粉末と混合するポリウレタン
は、平均分子量500〜2500のポリマージオール、例え
ば、ポリエステルジオール、ポリエーテルジオール、ポ
リエステルエーテルジオール、ポリカプロラクトンジオ
ール、ポリカーボネートジオールなどの群から選ばれた
少なくとも1種類のポリマージオールと、有機ポリイソ
シアネート、例えば、芳香族ジイソシアネート、芳香族
トリイソシアネート、脂環族ジイソシアネート、環状基
を有する脂肪族ジイソシアネート、トリフエニルメタン
4,4′,4″−トリイソシアネートなどの群から選ばれた
少なくとも1種類の有機ポリイソシアネートと、活性水
素原子を少なくとも2個有する低分子化合物を鎖伸長剤
として反応させて得たポリウレタンである。
In the present invention, the polyurethane mixed with the collagen powder is a polymer diol having an average molecular weight of 500 to 2500, for example, at least one selected from the group of polyester diol, polyether diol, polyester ether diol, polycaprolactone diol, polycarbonate diol and the like. And a polymer diol of an organic polyisocyanate such as an aromatic diisocyanate, an aromatic triisocyanate, an alicyclic diisocyanate, an aliphatic diisocyanate having a cyclic group, and triphenylmethane
Polyurethane obtained by reacting at least one organic polyisocyanate selected from the group of 4,4 ', 4 "-triisocyanate with a low molecular compound having at least two active hydrogen atoms as a chain extender. .

コラーゲンとポリウレタンを主体とした重合体の組成
物は、重合体の溶液にコラーゲン粉末が分散した分散液
として表面に塗布する。塗布液には目的に応じて染料や
顔料などの着色剤、安定剤、帯電防止剤、平滑剤などを
添加して用いる。塗布する方法は、例えば、刻目を有す
るロール、平滑面ロールなどのロールを用いて塗布する
ロール塗布法、スプレー塗布法、表面接触法などの方法
で塗布する。好ましい塗布方法は塗布の均一性や塗膜の
透気性、透湿性の高さの点からロール塗布法である。
A polymer composition mainly composed of collagen and polyurethane is applied to the surface as a dispersion in which collagen powder is dispersed in a polymer solution. Colorants such as dyes and pigments, stabilizers, antistatic agents, leveling agents, and the like are added to the coating solution depending on the purpose. As a method of applying, for example, a roll application method using a roll having a notch, a smooth surface roll, or the like, a coating method, a spray coating method, a surface contact method, or the like is used. A preferable coating method is a roll coating method from the viewpoint of uniformity of coating and high air permeability and moisture permeability of the coating film.

塗布量は、乾燥コラーゲンの重量にして5〜50g/m2
好ましくは5〜30g/m2の範囲である。コラーゲンの塗布
量が5g/m2より少ないと表面全体がコラーゲン粉末で覆
われないため、全体が徽目細かいマット調の表面となら
ず、また、サラッとしたタッチも得られない。コラーゲ
ンと塗布量が多いと外観はさほど悪化はしないものの皮
膜強度が低下し、耐久性に劣るものとなる。
The coating amount, 5 to 50 g / m 2 by weight of dry collagen,
Preferably in the range of 5 to 30 g / m 2. If the amount of collagen applied is less than 5 g / m 2 , the entire surface is not covered with the collagen powder, so that the entire surface does not have a fine matte surface and a smooth touch cannot be obtained. When the amount of collagen and the amount of coating are large, the appearance does not deteriorate so much, but the film strength is reduced and the durability is poor.

コラーゲンとポリウレタンを主体とした重合体の組成
物を付与された表面は、コラーゲン粒子の大きさとほぼ
同じ大きさの微細な凹凸を有する。この微細な凹凸によ
り光が散乱され、ギラツキのない徽目細かいマット調の
外観となる。コラーゲン粒子は重合体によって完全には
覆われておらず、コラーゲン粒子の多くはその一部が直
接表面に露出している。本発明の皮革様シートは、顔料
によっても着色することが出来るが、染色することによ
り色に一層の深みが出て好ましい。染色方法は、金属錯
塩染料、酸性染料、分散染料などを使用して、ウインス
染色法、ジッガー染色法などにより染色する。
The surface provided with the polymer composition mainly composed of collagen and polyurethane has fine irregularities having a size substantially equal to the size of the collagen particles. The light is scattered by the fine irregularities, and the appearance becomes a matte appearance without glare. Collagen particles are not completely covered by the polymer, and many of the collagen particles are directly exposed to the surface. The leather-like sheet of the present invention can be colored with a pigment, but it is preferable to dye the leather-like sheet because the color has more depth. As a dyeing method, a metal complex salt dye, an acid dye, a disperse dye, or the like is used, and dyeing is performed by a Wins dyeing method, a Jigger dyeing method, or the like.

本発明で得た皮革様シートは、良好な吸汗性を有し、
天然皮革のもつサラッとした質感と、天然皮革に類似の
ぬめり感のないスムースでナチュラルなタッチで見た目
に重厚感と色の深みがあり、徽目細かいマット調で濃く
見える。表面強度に優れた皮革様シートとなる。
The leather-like sheet obtained in the present invention has a good sweat-absorbing property,
It has the smooth texture of natural leather and the smooth, natural touch similar to natural leather without the slimy feel. It becomes a leather-like sheet with excellent surface strength.

本発明の皮革様シートは、スポーツシューズ、紳士靴
などの靴甲革、鞄、袋物、衣料、手袋などに使用するの
に適している。
The leather-like sheet of the present invention is suitable for use in shoe uppers such as sports shoes and men's shoes, bags, bags, clothing, gloves and the like.

<実施例> 次に、本発明の実施態様を具体的な実施例で説明する
が、本発明はこれら実施例に限定されるものではない。
なお、実施例中の部および%はことわりのない限り、重
量に関するものである。
<Examples> Next, embodiments of the present invention will be described with specific examples, but the present invention is not limited to these examples.
The parts and percentages in the examples relate to weight unless otherwise specified.

実施例1 基材シートとして、ポリエチレンテレフタレートを分
散成分、ポリエチレンを分散媒成分とする多成分繊維の
絡合不織布に、青系着色剤を含むポリエチレンアジペー
ト系ポリウレタンの20%ジメチルホルムアミド(DMF)
溶液を含浸し、更に表面に150g/m2の量塗布して40%DMF
水溶液中で凝固後ポリエチレンを溶解除去して得た極細
繊維束状繊維の不織布にポリウレタンが多孔質状態で含
有してなる基体層の一面にポリウレタン微多孔質表面層
を有するシートを用いた。この基材シートの表面に、ポ
リエステル系ポリウレタンの30%DMF溶液100部に平均粒
径5μm、見掛け嵩密度0.25g/cm3のコラーゲン粉末50
部および黒色顔料15部を添加した組成液をグラビアロー
ルを用いたロール塗布法により50g/m2となるよう塗布し
乾燥した。次いで、梨地模様のエンボスロールを用い、
湿度150℃で加熱エンボスを行い、金属錯塩染料により
染色後、更に機械揉みを行って皮革様シートAに仕上げ
た。
Example 1 20% dimethylformamide (DMF) of a polyethylene adipate-based polyurethane containing a blue-based coloring agent was used as a base sheet in an entangled nonwoven fabric of multicomponent fibers containing polyethylene terephthalate as a dispersion component and polyethylene as a dispersion medium component.
The solution was impregnated with, 40% DMF and further the amount applied of 150 g / m 2 on the surface
A sheet having a microporous polyurethane surface layer on one surface of a base layer in which polyurethane is contained in a porous state in a nonwoven fabric of ultrafine fiber bundles obtained by dissolving and removing polyethylene after coagulation in an aqueous solution was used. A collagen powder 50 having an average particle size of 5 μm and an apparent bulk density of 0.25 g / cm 3 was added to 100 parts of a 30% polyester polyurethane DMF solution on the surface of the base sheet.
And a composition liquid containing 15 parts by weight of a black pigment were applied by a roll coating method using a gravure roll to 50 g / m 2 and dried. Then, using a satin embossed roll,
Heat embossing was performed at a humidity of 150 ° C., and after dyeing with a metal complex dye, mechanical rubbing was further performed to complete the leather-like sheet A.

得られた皮革様シートAは風合いが柔らかで、良好な
吸汗性を有しており、天然皮革に類似のサラッとした質
感とぬめり感のないスムースでナチュラルなタッチを有
する触感であって、徽目の細かいマット調で天然皮革に
類似した深みのある黒度と見た目の重厚感を有するもの
であった。更に、表面の操作型電子顕微鏡で観察したと
ころ、コラーゲン粒子は半ばポリウレタンに埋まった状
態で微細な凹凸面を形成していた。
The obtained leather-like sheet A has a soft texture, a good sweat-absorbing property, a smooth texture similar to that of natural leather, and a tactile sensation having a smooth and natural touch without slimy feeling. It had a fine matte tone and had a deep blackness similar to natural leather and a solid appearance. Further, when the surface was observed with an operation-type electron microscope, it was found that the collagen particles had a fine uneven surface while being half-buried in polyurethane.

この皮革様シートAを用いて紳士靴および婦人靴を製
作したところ、カーフ様の柔軟な風合いでトップライン
がシャープに入り、高級感のあるものであった。
When the leather-like sheet A was used to produce men's shoes and women's shoes, the top line was sharp with a soft texture like a calf and had a high-class feel.

比較例1 実施例1において、コラーゲン粉末として平均粒径30
μm、見掛け嵩密度0.5g/cm3のコラーゲン粉末を用いる
以外は同様にして皮革様シートBに仕上げた。
Comparative Example 1 In Example 1, the average particle size was 30 as the collagen powder.
A leather-like sheet B was finished in the same manner except that collagen powder having a thickness of 0.5 μm and an apparent bulk density of 0.5 g / cm 3 was used.

皮革様シートBは、吸汗性はあるがザラツキ感のある
表面で、徽目が粗く、仕上げの悪いスエード調の外観で
あった。
The leather-like sheet B had a sweat-absorbing but rough surface, was rough in appearance, and had a poorly finished suede-like appearance.

実施例2 基材シートとして、繊度1.5デニールのポリエステル
短繊維の絡合不織布に実施例1と同様にポリエチレンア
ジペート系ポリウレタンを含浸・凝固して得たシートを
用いた。この基材シートの表面に、ポリエステル−エー
テル系ポリウレタンの30%DMF溶液100部に平均粒径7μ
m、見掛け嵩密度0.2g/cm3のコラーゲン粉末40部を添加
した組成液をグラビアロールを用いたロール塗布法によ
り40g/m2塗布し乾燥した。このシート状物の表面をカー
フ調模様のエンボスロールを用い、温度150℃で加熱エ
ンボスを行って皮革様シートCに仕上げた。
Example 2 As a substrate sheet, a sheet obtained by impregnating and coagulating a polyethylene adipate-based polyurethane in a woven nonwoven fabric of polyester short fibers having a fineness of 1.5 denier in the same manner as in Example 1 was used. On the surface of the base sheet, 100 parts of a 30% DMF solution of a polyester-ether polyurethane was added to an average particle diameter of 7 μm.
m, a composition solution to which 40 parts of collagen powder having an apparent bulk density of 0.2 g / cm 3 was added was applied at 40 g / m 2 by a roll coating method using a gravure roll, and dried. The surface of this sheet was heated and embossed at a temperature of 150 ° C. using a calf-like embossing roll to complete a leather-like sheet C.

得られた皮革様シートCは、適度の腰があり、表面は
徽目の細かいマット調で天然皮革のもつぬめりのないサ
ラッとした質感と、深みのある黒度を有していた。この
皮革様シートCを用いて紳士靴及びカメラケースを作製
したところ、いずれも賦型性および保型性に優れ、独特
のサラッとした触感と色調と相俟って商品価値の高いも
のであった。
The obtained leather-like sheet C had a moderate waist, had a fine matte tone on the surface, had a smooth texture without the sliminess of natural leather, and had a deep blackness. Using this leather-like sheet C, men's shoes and a camera case were produced, all of which were excellent in moldability and shape retention, and were of high commercial value combined with a unique smooth touch and color tone. Was.

実施例3 基材シートとして、6−ナイロンを分散媒成分、ポリ
スチレンを分散成分とする多成分繊維の絡合不織布に、
青系着色剤を含むポリエチレンアジペート系ポリウレタ
ンの20%ジメチルホルムアミド(DMF)溶液を含浸し、
更に表面に150g/m2の量塗布して40%DMF水溶液中で凝固
後ポリスチレンを溶解除去して得た特殊多孔繊維の不織
布にポリウレタンが多孔質状態で含有してなる基体層の
一面にポリウレタン微多孔質表面層を有するシートを用
いた。この基材シートの表面に、ポリエステル−エーテ
ル系ポリウレタンの30%DMF溶液100部に平均粒径7μ
m、見掛け嵩密度0.2g/cm3のコラーゲン粉末30部を添加
した組成液をグラビアロールを用いたロール塗布法によ
り40g/m2塗布し乾燥した。次いで、表面塗膜層面に梨地
模様のエンボスロールで加熱エンボスを行って皮革様シ
ートを得た。この皮革様シートは更に揉み処理して仕上
げた。
Example 3 As a base sheet, an entangled nonwoven fabric of multicomponent fibers containing 6-nylon as a dispersion medium component and polystyrene as a dispersion component,
Impregnated with a 20% dimethylformamide (DMF) solution of polyethylene adipate polyurethane containing a blue colorant,
In addition, a non-woven fabric of special porous fiber obtained by applying 150 g / m 2 on the surface and coagulating in a 40% DMF aqueous solution followed by dissolving and removing polystyrene, the polyurethane is contained in a porous state on one side of the base layer is polyurethane A sheet having a microporous surface layer was used. On the surface of the base sheet, 100 parts of a 30% DMF solution of a polyester-ether polyurethane was added to an average particle diameter of 7 μm.
m, a composition liquid to which 30 parts of collagen powder having an apparent bulk density of 0.2 g / cm 3 was added was applied at 40 g / m 2 by a roll coating method using a gravure roll, and dried. Next, heating embossing was performed on the surface coating layer with a satin embossing roll to obtain a leather-like sheet. This leather-like sheet was finished by further rubbing.

得られた皮革様シートは見た目の重厚感があるが手に
持つと軽量て、表面はサラッとして徽目細かいマット調
で深みのある黒度があり、学振型平面摩耗試験器による
荷重500g、回数1000回の摩耗試験後も異状なしであっ
た。
The obtained leather-like sheet has a profound feeling of appearance, but it is light when held in hand, the surface is smooth and has a fine matte tone with a deep blackness, a load of 500 g by Gakushin type flat wear tester, No abnormalities were observed after the abrasion test 1000 times.

この皮革様シートは鞄やランドセル、スポーツシュー
ズ用として好適の素材であった。
This leather-like sheet was a suitable material for bags, school bags, and sports shoes.

<発明の効果> 本発明の皮革様シートは、手に濡れた感触が天然皮革
のような汗を吸い込むようなぬめり感のないサラッとし
た質感及び良好な吸汗性を有し、天然皮革に類似した見
た目の重厚感と色の深みがあり、かつ徽目の細かいマッ
ト調で濃く見える、表面強さに優れた皮革様シートであ
る。
<Effects of the Invention> The leather-like sheet of the present invention has a smooth texture and a good sweat-absorbing property without the slimy feeling that the wet feeling of the hand sucks sweat like natural leather, and is similar to natural leather. It is a leather-like sheet with excellent surface strength, which has a solid appearance and depth of color, and looks dark with a fine matte tone.

───────────────────────────────────────────────────── フロントページの続き (58)調査した分野(Int.Cl.6,DB名) D06N 3/14 B32B 27/40──────────────────────────────────────────────────続 き Continued on front page (58) Field surveyed (Int.Cl. 6 , DB name) D06N 3/14 B32B 27/40

Claims (1)

(57)【特許請求の範囲】(57) [Claims] 【請求項1】繊維集合体に弾性重合体を主体とした重合
体を含有した基体層と弾性重合体を主体とした重合体の
被覆層とからなる皮革様シートにおいて、該被覆層の表
面が非繊維状で平均粒径10μ以下かつ見掛け嵩密度0.1
〜0.3g/cm3のコラーゲン粉末とポリウレタンを主体とし
た重合体との混合物よりなり微細な凹凸を有することを
特徴とする皮革様シート。
A leather-like sheet comprising a base layer containing a polymer mainly composed of an elastic polymer in a fiber aggregate and a coating layer of a polymer mainly composed of an elastic polymer, wherein the surface of the coating layer is Non-fibrous, average particle size 10μ or less and apparent bulk density 0.1
A leather-like sheet comprising a mixture of collagen powder of about 0.3 g / cm 3 and a polymer mainly composed of polyurethane and having fine irregularities.
JP8540690A 1990-03-30 1990-03-30 Leather-like sheet Expired - Fee Related JP2809803B2 (en)