JP2010006922A - Polycarbonate resin composition and molded article comprising it - Google Patents
Polycarbonate resin composition and molded article comprising it Download PDFInfo
- Publication number
- JP2010006922A JP2010006922A JP2008166777A JP2008166777A JP2010006922A JP 2010006922 A JP2010006922 A JP 2010006922A JP 2008166777 A JP2008166777 A JP 2008166777A JP 2008166777 A JP2008166777 A JP 2008166777A JP 2010006922 A JP2010006922 A JP 2010006922A
- Authority
- JP
- Japan
- Prior art keywords
- polycarbonate resin
- resin composition
- oligomer
- acid ester
- molded article
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
Description
本発明は、ポリカーボネート樹脂に環状ポリ(アルキレンテレフタレート)オリゴマーおよびグリセリン脂肪酸エステルを配合することにより、流動性および摺動性(耐引掻き性)を向上させたポリカーボネート樹脂組成物、ならびにそれからなる成形品に関する。 The present invention relates to a polycarbonate resin composition having improved fluidity and slidability (scratch resistance) by incorporating a cyclic poly (alkylene terephthalate) oligomer and a glycerin fatty acid ester into a polycarbonate resin, and a molded article comprising the same. .
ポリカーボネート樹脂は、耐衝撃性、透明性、耐熱性、熱安定性等に優れた熱可塑性樹脂であり、電気、電子、ITE、機械、自動車などの分野で広く用いられている。一方、当該樹脂が有するこれらの優れた性能に加えて、前述の各分野では、意匠面やデザイン上の要求を満たすため、高度な流動性(成形性)を具備した材料が求められている。特に近年では、製品の軽量化の傾向が著しく、ポリカーボネート樹脂に対する流動性改善の要求はますます顕著化しているのがその実態である。 Polycarbonate resin is a thermoplastic resin excellent in impact resistance, transparency, heat resistance, thermal stability and the like, and is widely used in fields such as electricity, electronics, ITE, machinery, and automobiles. On the other hand, in addition to these excellent performances of the resin, in each of the aforementioned fields, a material having a high fluidity (moldability) is required in order to satisfy the design and design requirements. In particular, in recent years, the trend of weight reduction of products has been remarkable, and the actual situation is that the demand for improvement in fluidity of polycarbonate resins has become more prominent.
一方、当該ポリカーボネート樹脂の流動性を改善させる手法として、過去より様々な技術が提案されてきたが、いずれも一長一短があり、必ずしも満足できる材料が提案されているわけではない。
前述したようにポリカーボネート樹脂の流動性を改善する一般的な方法として、低分子可塑剤等低分子量の化合物や良流動性のポリマー等を配合する技術が提案されているが、これらの技術では、ポリカーボネート樹脂が持つ前述の優れた特徴の内いずれか1種以上が大きく損なわれてしまうといった問題を孕んでおり、従来からその改善が強く望まれてきた。 As described above, as a general method for improving the fluidity of the polycarbonate resin, a technique of blending a low molecular weight compound such as a low molecular plasticizer or a good fluidity polymer has been proposed. There is a problem that any one or more of the above-described excellent characteristics of the polycarbonate resin is greatly impaired, and there has been a strong demand for improvement thereof.
本発明者らは、かかる問題点に鑑み鋭意検討を行った結果、当該ポリカーボネート樹脂組成物に、特定の環状ポリ(アルキレンテレフタレート)オリゴマーおよびグリセリン脂肪酸エステルを特定量併用して配合することにより、ポリカーボネート樹脂の流動性および摺動性(耐引掻き性)を顕著に改善することに成功し、本発明に到達したものである。 As a result of intensive studies in view of such problems, the present inventors have formulated a polycarbonate by combining a specific cyclic poly (alkylene terephthalate) oligomer and a glycerin fatty acid ester in a specific amount in combination with the polycarbonate resin composition. The present inventors have succeeded in remarkably improving the fluidity and slidability (scratch resistance) of the resin and have reached the present invention.
すなわち、本発明は、ポリカーボネート樹脂(A)100重量部、環状ポリ(アルキレンテレフタレート)オリゴマー(B)0.5〜6重量部およびグリセリン脂肪酸エステル(C)0.01〜1重量部からなることを特徴とするポリカーボネート樹脂組成物、ならびにそれからなる成形品を提供するものである。 That is, the present invention comprises 100 parts by weight of polycarbonate resin (A), 0.5 to 6 parts by weight of cyclic poly (alkylene terephthalate) oligomer (B) and 0.01 to 1 part by weight of glycerin fatty acid ester (C). It is intended to provide a polycarbonate resin composition and a molded article comprising the polycarbonate resin composition.
本発明は、ポリカーボネート樹脂が本来有する優れた衝撃強度、耐熱性、熱安定性等の性能を維持したまま流動性および摺動性(耐引掻き性)を顕著に改善させ得る技術であり、得られたポリカーボネート樹脂組成物は電機、電子、ITE等各種分野における製品の筐体や部品として好適に使用することが可能であって、工業的利用価値が極めて高い。 The present invention is a technique that can remarkably improve the fluidity and slidability (scratch resistance) while maintaining the excellent impact strength, heat resistance, thermal stability and the like inherent to the polycarbonate resin. The polycarbonate resin composition can be suitably used as a housing or part of a product in various fields such as electrical machinery, electronics, and ITE, and has an extremely high industrial utility value.
本発明にて使用されるポリカーボネート樹脂(A)とは、種々のジヒドロキシジアリール化合物とホスゲンとを反応させるホスゲン法、またはジヒドロキシジアリール化合物とジフェニルカーボネートなどの炭酸エステルとを反応させるエステル交換法によって得られる重合体であり、代表的なものとしては、2,2−ビス(4−ヒドロキシフェニル)プロパン(ビスフェノールA)から製造されたポリカーボネート樹脂が挙げられる。 The polycarbonate resin (A) used in the present invention is obtained by a phosgene method in which various dihydroxydiaryl compounds and phosgene are reacted, or a transesterification method in which a dihydroxydiaryl compound and a carbonate such as diphenyl carbonate are reacted. A typical example of the polymer is a polycarbonate resin produced from 2,2-bis (4-hydroxyphenyl) propane (bisphenol A).
上記ジヒドロキシジアリール化合物としては、ビスフェノールAの他に、ビス(4−ヒドロキシフェニル)メタン、1,1−ビス(4−ヒドロキシフェニル)エタン、2,2−ビス(4−ヒドロキシフェニル)ブタン、2,2−ビス(4−ヒドロキシフェニル)オクタン、ビス(4−ヒドロキシフェニル)フェニルメタン、2,2−ビス(4−ヒドロキシフェニル−3−メチルフェニル)プロパン、1,1−ビス(4−ヒドロキシ−3−第三ブチルフェニル)プロパン、2,2−ビス(4−ヒドロキシ−3−ブロモフェニル)プロパン、2,2−ビス(4−ヒドロキシ−3、5−ジブロモフェニル)プロパン、2,2−ビス(4−ヒドロキシ−3,5−ジクロロフェニル)プロパンのようなビス(ヒドロキシアリール)アルカン類、1,1−ビス(4−ヒドロキシフェニル)シクロペンタン、1,1−ビス(4−ヒドロキシフェニル)シクロヘキサンのようなビス(ヒドロキシアリール)シクロアルカン類、4,4′−ジヒドロキシジフェニルエーテル、4,4′−ジヒドロキシ−3,3′−ジメチルジフェニルエーテルのようなジヒドロキシジアリールエーテル類、4,4′−ジヒドロキシジフェニルスルフィドのようなジヒドロキシジアリールスルフィド類、4,4′−ジヒドロキシジフェニルスルホキシド、4,4′−ジヒドロキシ−3,3′−ジメチルジフェニルスルホキシドのようなジヒドロキシジアリールスルホキシド類、4,4′−ジヒドロキシジフェニルスルホン、4,4′−ジヒドロキシ−3,3′−ジメチルジフェニルスルホンのようなジヒドロキシジアリールスルホン類等が挙げられる。これらは、単独または2種類以上混合して使用される。これらの他に、ピペラジン、ジピペリジルハイドロキノン、レゾルシン、4,4′−ジヒドロキシジフェニル等を混合して使用してもよい。 Examples of the dihydroxydiaryl compound include bisphenol 4-, bis (4-hydroxyphenyl) methane, 1,1-bis (4-hydroxyphenyl) ethane, 2,2-bis (4-hydroxyphenyl) butane, 2, 2-bis (4-hydroxyphenyl) octane, bis (4-hydroxyphenyl) phenylmethane, 2,2-bis (4-hydroxyphenyl-3-methylphenyl) propane, 1,1-bis (4-hydroxy-3) -Tert-butylphenyl) propane, 2,2-bis (4-hydroxy-3-bromophenyl) propane, 2,2-bis (4-hydroxy-3,5-dibromophenyl) propane, 2,2-bis ( Bis (hydroxyaryl) alkanes such as 4-hydroxy-3,5-dichlorophenyl) propane, 1,1- (4-hydroxyphenyl) cyclopentane, bis (hydroxyaryl) cycloalkanes such as 1,1-bis (4-hydroxyphenyl) cyclohexane, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxy-3 Dihydroxy diaryl ethers such as 3,3'-dimethyldiphenyl ether, dihydroxy diaryl sulfides such as 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxydiphenyl sulfoxide, 4,4'-dihydroxy-3,3 ' Dihydroxy diaryl sulfoxides such as dimethyldiphenyl sulfoxide, dihydroxy diary such as 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfone Sulfone, and the like. These are used individually or in mixture of 2 or more types. In addition to these, piperazine, dipiperidyl hydroquinone, resorcin, 4,4'-dihydroxydiphenyl, and the like may be mixed and used.
さらに、上記のジヒドロキシアリール化合物と以下に示すような3価以上のフェノール化合物を混合使用してもよい。3価以上のフェノールとしてはフロログルシン、4,6−ジメチル−2,4,6−トリ−(4−ヒドロキシフェニル)−ヘプテン、2,4,6−ジメチル−2,4,6−トリ−(4−ヒドロキシフェニル)−ヘプタン、1,3,5−トリ−(4−ヒドロキシフェニル)−ベンゾール、1,1,1−トリ−(4−ヒドロキシフェニル)−エタンおよび2,2−ビス−[4,4−(4,4′−ジヒドロキシジフェニル)−シクロヘキシル]−プロパンなどが挙げられる。 Furthermore, the above dihydroxyaryl compound and a trivalent or higher phenol compound as shown below may be used in combination. Trihydric or higher phenols include phloroglucin, 4,6-dimethyl-2,4,6-tri- (4-hydroxyphenyl) -heptene, 2,4,6-dimethyl-2,4,6-tri- (4 -Hydroxyphenyl) -heptane, 1,3,5-tri- (4-hydroxyphenyl) -benzol, 1,1,1-tri- (4-hydroxyphenyl) -ethane and 2,2-bis- [4 4- (4,4'-dihydroxydiphenyl) -cyclohexyl] -propane and the like.
ポリカーボネート樹脂(A)の粘度平均分子量は、通常10000〜100000、好ましくは15000〜35000、さらに好ましくは17000〜28000である。かかるポリカーボネート樹脂を製造するに際し、分子量調節剤、触媒等を必要に応じて使用することができる。 The viscosity average molecular weight of the polycarbonate resin (A) is usually 10,000 to 100,000, preferably 15,000 to 35,000, and more preferably 17,000 to 28,000. In producing such a polycarbonate resin, a molecular weight regulator, a catalyst and the like can be used as necessary.
本発明にて使用される環状ポリ(アルキレンテレフタレート)オリゴマー(B)は、下記一般式に示される構成単位を有するものをいう。 The cyclic poly (alkylene terephthalate) oligomer (B) used in the present invention refers to one having a structural unit represented by the following general formula.
式中、Rは炭素数2〜8のアルキレン基、Arは2価の芳香族基を表す。とりわけ、Rがエチレンまたはテトラメチレンであり、Arがm−フェニレンまたはp−フェニレンであるものが好ましく使用される。 In the formula, R represents an alkylene group having 2 to 8 carbon atoms, and Ar represents a divalent aromatic group. In particular, those in which R is ethylene or tetramethylene and Ar is m-phenylene or p-phenylene are preferably used.
環状ポリ(アルキレンテレフタレート)オリゴマー(B)は、通常、重合度2〜30の重合度のオリゴマーからなり、その主要成分が12までの重合度を有する環状オリゴマーの混合物である。市販品としては、サイクリクスコーポレーション社製CBTがあげられる。 The cyclic poly (alkylene terephthalate) oligomer (B) is usually a mixture of cyclic oligomers having a polymerization degree of 2 to 30 and the main component having a polymerization degree of up to 12. Commercially available products include CBT manufactured by Cyclix Corporation.
環状ポリ(アルキレンテレフタレート)オリゴマー(B)の配合量は、ポリカーボネート樹脂(A)100重量部に対し、0.5〜6重量部である。配合量が0.5重量部未満では流動性の向上効果が小さく、6重量部を超えると成形時にガス発生量が多くなり、金型汚れが発生したり、成形品の外観が低下するので好ましくない。より好ましくは、3〜5重量部の範囲である。 The compounding quantity of cyclic poly (alkylene terephthalate) oligomer (B) is 0.5-6 weight part with respect to 100 weight part of polycarbonate resin (A). If the blending amount is less than 0.5 parts by weight, the effect of improving the fluidity is small, and if it exceeds 6 parts by weight, the amount of gas generation increases during molding, mold fouling occurs, and the appearance of the molded product is reduced, which is preferable. Absent. More preferably, it is in the range of 3 to 5 parts by weight.
本発明にて使用されるグリセリン脂肪酸エステル(C)とは、グリセリンと炭素数が20以上の脂肪酸とのエステルである。炭素数が20以上の脂肪酸としては、アラキン酸、ベヘン酸、リグノセリン酸、セロチン酸、ヘプタコサン酸、モンタン酸、メリシン酸、ラクセル酸などが挙げられる。これらの炭素数が20以上の脂肪酸とグリセリンとのモノエステルが好適に使用され、特にグリセリンモノベヘネートが好適に使用される。炭素数が20未満の脂肪酸からなるグリセリン脂肪酸エステルを用いた場合、成形品の外観や熱安定性が著しく劣り、また衝撃強度も低下する傾向にあるので好ましくない。 The glycerin fatty acid ester (C) used in the present invention is an ester of glycerin and a fatty acid having 20 or more carbon atoms. Examples of the fatty acid having 20 or more carbon atoms include arachidic acid, behenic acid, lignoceric acid, serotic acid, heptacosanoic acid, montanic acid, melicic acid, and laccelic acid. Monoesters of these fatty acids having 20 or more carbon atoms and glycerol are preferably used, and glycerol monobehenate is particularly preferably used. When a glycerin fatty acid ester composed of a fatty acid having less than 20 carbon atoms is used, the appearance and thermal stability of the molded product are remarkably inferior, and the impact strength tends to decrease.
グリセリン脂肪酸エステル(C)の配合量は、ポリカーボネート樹脂(A)100重量部に対し、0.01〜1重量部である。配合量が0.01重量部未満であると摺動性(耐引掻き性)に劣り、配合量が1重量部を越えると熱安定性、耐衝撃性に劣るので好ましくない。より好ましくは0.1〜0.5重量部である。 The compounding quantity of glycerol fatty acid ester (C) is 0.01-1 weight part with respect to 100 weight part of polycarbonate resin (A). If the amount is less than 0.01 parts by weight, the sliding property (scratch resistance) is inferior, and if the amount exceeds 1 part by weight, the thermal stability and impact resistance are inferior. More preferably, it is 0.1-0.5 weight part.
本発明のポリカーボネート樹脂組成物において、実用上、要求される性能により、公知の各種添加剤、ポリマーなどを必要に応じて添加することができる。例えば、長期間、光に暴露された際の樹脂成形品の変色を抑制するために、ヒンダードアミン系の耐光安定剤、ベンゾトリアゾール系、ベンゾフェノン系、トリアジン系およびマロネート系の紫外線吸収剤およびこれらを併用して添加してもよい。 In the polycarbonate resin composition of the present invention, various known additives, polymers, and the like can be added as necessary depending on the performance required for practical use. For example, in order to suppress discoloration of resin molded products when exposed to light for a long period of time, a hindered amine light-resistant stabilizer, a benzotriazole-based, benzophenone-based, triazine-based, and malonate-based UV absorber and a combination thereof are used. May be added.
また、難燃性が必要とされる場合、公知の各種難燃剤、例えば、テトラブロモビスフェノールAオリゴマーなどの臭素系難燃剤、トリフェニルホスフェート、トリクレジルホスフェートなどのモノリン酸エステル類、ビスフェノールAジホスフェート、レゾルシンジホスフェート、テトラキシレニルレゾルシンジホスフェートなどオリゴマータイプの縮合リン酸エステル類、ポリリン酸アンモニウムおよび赤燐などのリン系難燃剤、各種シリコーン系難燃剤、あるいは難燃性をより高めるために、芳香族スルホン酸の金属塩、パーフルオロアルカンスルホン酸の金属塩があげられ、好適には、4−メチル−N−(4−メチルフェニル)スルフォニル−ベンゼンスルフォンアミドのカリウム塩、ジフェニルスルホン−3−スルホン酸カリウム、ジフェニルスルホン−3−3′−ジスルホン酸カリウム、パラトルエンスルホン酸ナトリウム、パーフルオロブタンスルホン酸カリウム塩等などの有機金属塩なども添加することができる。これらの難燃剤の中でも、リン系難燃剤は、難燃性を向上させるばかりでなく、流動性をも向上させることができることから好適に用いることができる。 When flame retardancy is required, various known flame retardants, for example, brominated flame retardants such as tetrabromobisphenol A oligomers, monophosphate esters such as triphenyl phosphate and tricresyl phosphate, bisphenol A diesters, etc. In order to further improve the flame retardancy, phosphorous flame retardants such as phosphate-type condensed phosphates such as phosphate, resorcin diphosphate, tetraxylenyl resorcin diphosphate, ammonium polyphosphate and red phosphorus, various silicone flame retardants And metal salts of aromatic sulfonic acid and perfluoroalkanesulfonic acid, preferably 4-methyl-N- (4-methylphenyl) sulfonyl-benzenesulfonamide potassium salt, diphenylsulfone- 3- potassium sulfonate, Potassium phenyl sulfonic -3-3'- disulfonic acid, sodium para-toluene sulfonic acid, also organic metal salts such as potassium perfluorobutane sulfonate and the like may be added. Among these flame retardants, phosphorus-based flame retardants can be suitably used because they can improve not only flame retardancy but also fluidity.
本発明のポリオカーボネート樹脂組成物には、上記以外の公知の添加剤、例えばフェノール系またはリン系熱安定剤[2,6−ジ−t−ブチル−4−メチルフェノール、2−(1−メチルシクロヘキシル)−4,6−ジメチルフェノール、4,4′−チオビス−(6−t−ブチル−3−メチルフェノール)、2,2−メチレンビス−(4−エチル−6−t−メチルフェノール)、n−オクタデシル−3−(3,5−ジ−t−ブチル−4−ヒドロキシフェニル)プロピオネート、トリス(2,4−ジ−t−ブチルフェニル)フォスファイト、4,4′−ビフェニレンジホスフィン酸テトラキス−(2,4−ジ−t−ブチルフェニル)等]、滑剤[パラフィンワックス、n−ブチルステアレート、合成蜜蝋、天然蜜蝋、グリセリンモノエステル、モンタン酸ワックス、ポリエチレンワックス、ペンタエリスリトールテトラステアレート等]、着色剤[例えば酸化チタン、カーボンブラック、染料]、充填剤[炭酸カルシウム、クレー、シリカ、ガラス繊維、ガラス球、ガラスフレーク、カーボン繊維、タルク、マイカ、各種ウィスカー類等]、流動性改良剤、展着剤[エポキシ化大豆油、流動パラフィン等]、さらには他の熱可塑性樹脂や各種耐衝撃改良剤(ポリブタジエン、ポリアクリル酸エステル、エチレン・プロピレン系ゴム等のゴムに、メタアクリル酸エステル、スチレン、アクリロニトリル等の化合物をグラフト重合してなるゴム強化樹脂等が例示される。)を必要に応じて添加することができる。 In the polycarbonate resin composition of the present invention, known additives other than those described above, for example, phenol-based or phosphorus-based heat stabilizer [2,6-di-t-butyl-4-methylphenol, 2- (1-methyl Cyclohexyl) -4,6-dimethylphenol, 4,4'-thiobis- (6-tert-butyl-3-methylphenol), 2,2-methylenebis- (4-ethyl-6-tert-methylphenol), n -Octadecyl-3- (3,5-di-t-butyl-4-hydroxyphenyl) propionate, tris (2,4-di-t-butylphenyl) phosphite, 4,4'-biphenylenediphosphinic acid tetrakis- ( 2,4-di-t-butylphenyl), etc.], lubricant [paraffin wax, n-butyl stearate, synthetic beeswax, natural beeswax, glycerin monoester, Tantalate wax, polyethylene wax, pentaerythritol tetrastearate, etc.], colorant [eg titanium oxide, carbon black, dye], filler [calcium carbonate, clay, silica, glass fiber, glass sphere, glass flake, carbon fiber, Talc, mica, various whiskers, etc.], fluidity improvers, spreading agents [epoxidized soybean oil, liquid paraffin, etc.], other thermoplastic resins and various impact resistance improvers (polybutadiene, polyacrylate, A rubber reinforced resin obtained by graft polymerization of a compound such as methacrylic acid ester, styrene, acrylonitrile, etc. to a rubber such as an ethylene / propylene rubber may be added as necessary.
本発明における実施の形態および順序には何ら制限はない。例えば、ポリカーボネート樹脂(A)、環状ポリ(アルキレンテレフタレート)オリゴマー(B)およびグリセリン脂肪酸エステル(C)を任意の配合量で計量し、タンブラー、リボブレンダー、高速ミキサー等により一括混合した後、混合物を通常の一軸またはニ軸押出機を用いて溶融混練し、ペレット化させる方法、あるいは、各々の成分を一部または全てを別々に計量し、複数の供給装置から押出機内へ投入し、溶融混合する方法、さらには、(A)に(B)および/または(C)を高濃度に配合し、一旦溶融混合してペレット化し、マスターバッチとした後、当該マスターバッチと(A)を、所望の比率により混合することもできる。そして、これらの成分を溶融混合する際の、押出機の投入する位置、押出温度、スクリュー回転数、供給量など、状況に応じて任意の条件が選択され、ペレット化することができる。さらに、該マスターバッチと(A)とを、所望の比率により乾式混合後、射出成形装置やシート押出機装置に直接投入し、成形品とすることも可能である。 There is no restriction | limiting in the embodiment and order in this invention. For example, a polycarbonate resin (A), a cyclic poly (alkylene terephthalate) oligomer (B), and a glycerin fatty acid ester (C) are weighed in arbitrary blending amounts and mixed together using a tumbler, riboblender, high-speed mixer, etc. Melting and kneading using an ordinary single-screw or twin-screw extruder and pelletizing, or partially or all of each component is separately weighed, introduced into the extruder from a plurality of feeders, and melt mixed The method, and further, (B) and / or (C) is blended at a high concentration in (A), once melt-mixed and pelletized to obtain a master batch, and then the master batch and (A) are mixed in a desired manner. It can also be mixed in proportions. Then, when these components are melt-mixed, arbitrary conditions such as the position at which the extruder is introduced, the extrusion temperature, the screw rotation speed, the supply amount, and the like can be selected and pelletized. Further, the master batch and (A) can be mixed by dry mixing at a desired ratio, and then directly fed into an injection molding apparatus or a sheet extruder apparatus to form a molded product.
以下、本発明を実施例により説明するが、本発明はその要旨を超えない限りこれら実施例に限定されるものではない。尚、特に断りのない限り、実施例中の「%」、「部」はそれぞれ重量基準に基づく。 EXAMPLES Hereinafter, although an Example demonstrates this invention, this invention is not limited to these Examples, unless the summary is exceeded. Unless otherwise specified, “%” and “part” in the examples are based on weight standards.
尚、使用された各種配合成分は以下のものである。
ポリカーボネート樹脂:
住友ダウ社製カリバー200−20
(粘度平均分子量:18500、以下PCと略記)
環状ポリ(ブチレンテレフタレート)オリゴマー:
サイクリクスコーポレーション社製CBT
(融点140〜190℃、以下CBTと略記)
グリセリン脂肪酸エステル:
理研ビタミン社製 リケマール B−100(以下、GFAEと略記)
(グリセリンモノベヘネート;脂肪酸の炭素数22)
In addition, the various compounding components used are as follows.
Polycarbonate resin:
Sumitomo Dow Caliber 200-20
(Viscosity average molecular weight: 18500, hereinafter abbreviated as PC)
Cyclic poly (butylene terephthalate) oligomer:
CBT made by Cyclix Corporation
(Melting point: 140 to 190 ° C., hereinafter abbreviated as CBT)
Glycerin fatty acid ester:
Rikenmar B-100 manufactured by Riken Vitamin (hereinafter abbreviated as GFAE)
(Glycerin monobehenate; fatty acid 22 carbon atoms)
前述の各種原料を表1〜2に示す配合比率にて一括してタンブラーに投入し、10分間乾式混合した後、二軸押出機(神戸製鋼所製KTX37)を用いて、溶融温度280℃にて混練し、ポリカーボネート樹脂組成物のペレットを得た。得られたペレットから、日本製鋼所製・J100E−C5射出成形機を用いて各種試験片を加工し、下記方法により各種データーを採取した。 The above-mentioned various raw materials are collectively put into a tumbler at the blending ratios shown in Tables 1-2, and after dry mixing for 10 minutes, using a twin screw extruder (KTX37 manufactured by Kobe Steel), the melting temperature is 280 ° C. And kneaded to obtain pellets of the polycarbonate resin composition. Various test pieces were processed from the obtained pellets using a J100E-C5 injection molding machine manufactured by Nippon Steel Works, and various data were collected by the following methods.
(アルキメデススパイラルフロー流動性)
溶融温度280℃、射出圧力1600kg/cm2の条件下、アルキメデススパイラルフロー金型を使用して、流路厚み1mmでの流動長さを測定した。流動長さが125mm以上を合格とした。
(Archimedes spiral flow fluidity)
The flow length at a channel thickness of 1 mm was measured using an Archimedes spiral flow mold under the conditions of a melting temperature of 280 ° C. and an injection pressure of 1600 kg / cm 2 . A flow length of 125 mm or more was regarded as acceptable.
(アイゾット衝撃強度)
溶融温度280℃の条件下、アイゾット衝撃試験用試験片を加工し、ASTM D256に準拠し、アイゾット衝撃強度を測定した。測定温度は23℃、試験片の厚みは3.2mmである。衝撃値が20Kg・cm/cm以上を合格とした。
(Izod impact strength)
A specimen for an Izod impact test was processed under the condition of a melting temperature of 280 ° C., and the Izod impact strength was measured in accordance with ASTM D256. The measurement temperature is 23 ° C., and the thickness of the test piece is 3.2 mm. An impact value of 20 kg / cm / cm or more was considered acceptable.
(静摩擦係数)
得られた試験片(150x90x3mm)を用いて、JIS K7125に準拠して、
摩擦係数測定機(テスター産業社製AB−401)を使用して静摩擦係数を測定した。
1以下を合格とした。
(Static friction coefficient)
Using the obtained test piece (150x90x3mm), in accordance with JIS K7125,
The static friction coefficient was measured using a friction coefficient measuring machine (AB-401, manufactured by Tester Sangyo Co., Ltd.).
1 or less was accepted.
表1のとおり、ポリカーボネート樹脂組成物が本発明の構成要件を満足する場合(実施例1〜5)にあっては、全ての評価項目にわたりその規格を満足していた。 As shown in Table 1, when the polycarbonate resin composition satisfied the constituent requirements of the present invention (Examples 1 to 5), the standard was satisfied over all evaluation items.
表2で示したとおり、ポリカーボネート樹脂組成物が本発明の構成要件を満足しない場合においては、いずれの場合も何らかの欠点を有していた。
比較例1は、CBTの配合量が規定範囲の下限より少ない場合で、流動性に劣っていた。
比較例2は、CBTの配合量が規定範囲の上限より多い場合で、衝撃強度に劣っていた。
比較例3は、GFAEの配合量が規定範囲の下限より少ない場合で、摺動性に劣っていた。
比較例4は、GFAEの配合量が規定範囲の上限より多い場合で、衝撃強度に劣っていた。
As shown in Table 2, when the polycarbonate resin composition did not satisfy the constituent requirements of the present invention, each case had some drawbacks.
In Comparative Example 1, the blending amount of CBT was less than the lower limit of the specified range, and the fluidity was inferior.
In Comparative Example 2, the amount of CBT was greater than the upper limit of the specified range, and the impact strength was inferior.
Comparative Example 3 was inferior in slidability when the amount of GFAE was less than the lower limit of the specified range.
In Comparative Example 4, the amount of GFAE was greater than the upper limit of the specified range, and the impact strength was inferior.
Claims (5)
とする請求項1記載のポリカーボネート樹脂組成物。 The polycarbonate resin composition according to claim 1, wherein the glycerin fatty acid ester (C) is glycerin monobehenate.
The polycarbonate resin composition according to claim 1.