JP2005240087A - Briquette for raw material for steelmaking and method for manufacturing the same - Google Patents

Briquette for raw material for steelmaking and method for manufacturing the same Download PDF

Info

Publication number
JP2005240087A
JP2005240087A JP2004050197A JP2004050197A JP2005240087A JP 2005240087 A JP2005240087 A JP 2005240087A JP 2004050197 A JP2004050197 A JP 2004050197A JP 2004050197 A JP2004050197 A JP 2004050197A JP 2005240087 A JP2005240087 A JP 2005240087A
Authority
JP
Japan
Prior art keywords
shot
briquette
grinding
raw material
oil
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP2004050197A
Other languages
Japanese (ja)
Inventor
Mitsuma Matsuda
光馬 松田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Koyo Seiko Co Ltd
Original Assignee
Koyo Seiko Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Koyo Seiko Co Ltd filed Critical Koyo Seiko Co Ltd
Priority to JP2004050197A priority Critical patent/JP2005240087A/en
Priority to US10/589,963 priority patent/US20070163389A1/en
Priority to CNB2005800056275A priority patent/CN100537795C/en
Priority to EP05719514A priority patent/EP1726666A4/en
Priority to PCT/JP2005/003113 priority patent/WO2005080614A1/en
Publication of JP2005240087A publication Critical patent/JP2005240087A/en
Pending legal-status Critical Current

Abstract

<P>PROBLEM TO BE SOLVED: To provide a method for manufacturing briquettes for a raw material for steelmaking in which shot residue can be effectively recycled, and to provide a method for manufacturing the same. <P>SOLUTION: Grinding sludge B which contains grinding-wheel swarf of ferrous metal and grinding fluid containing oil and water is mixed with shot residue S to obtain a flocculent agglomerate M. The flocculent agglomerate M is compacted to prepare a brittle compact C where the grinding-wheel swarf in a fibrous state is roughly sheared and excess water and oil are removed. The brittle compact B is impregnated with an auxiliary agent D for solidification to undergo solidification, followed by drying. <P>COPYRIGHT: (C)2005,JPO&NCIPI

Description

この発明は、製鋼原料用のブリケット及びその製造方法に関し、特に、鉄系金属にショットブラストを施した際に生じるショット粕を有効利用する技術に関する。   The present invention relates to a briquette for a steelmaking raw material and a method for producing the same, and more particularly to a technique for effectively using shot soot generated when shot blasting is performed on an iron-based metal.

軸受鋼や浸炭鋼等の鉄系金属を研削(以下研磨、超仕上げ研磨及びラッピング等も含む概念として使用する)した際に生じる切粉は、水分及び油分を含有する研削液や砥粒等を含む綿状(繊維状)の研削スラッジとして回収されている。この研削スラッジは、多量の純鉄を含むことからこれを製鋼原料として再利用することが試みられている。例えば、特許文献1には、前記研削スラッジを圧縮成形した後、固形化補助剤を含浸させて、製鋼原料用のブリケットとして再利用する技術が開示されている。
一方、鉄系金属にショットブラスを施した際に生じるショット粕については、一般に鉄粉と使用済のショット玉(鋼球)とを含んでいるので、製鋼原料として有効な資源となり得る。しかしながら、このショット粕は発火したり飛散したりし易いので、運搬、貯蔵等の取り扱いが困難であるとともに、再利用するには技術的にもコスト的にも不利である。このため、前記ショット粕は産業廃棄物として埋め立て処分されているのが実情である。
特開2002−129248号公報(図1)
Chips generated when grinding ferrous metals such as bearing steel and carburized steel (hereinafter used as a concept that includes polishing, superfinishing polishing, lapping, etc.) are used for grinding fluids and abrasives containing moisture and oil. It is recovered as a cotton-like (fibrous) grinding sludge. Since this grinding sludge contains a large amount of pure iron, it has been attempted to reuse it as a raw material for steelmaking. For example, Patent Document 1 discloses a technique in which the grinding sludge is compression-molded and then impregnated with a solidification auxiliary and reused as a briquette for a steelmaking raw material.
On the other hand, since the shot soot produced when shot brass is applied to an iron-based metal generally contains iron powder and used shot balls (steel balls), it can be an effective resource as a steelmaking raw material. However, since this shot soot is easy to ignite or scatter, handling such as transportation and storage is difficult, and it is disadvantageous in terms of technology and cost to reuse. For this reason, the actual situation is that the shot culvert is disposed of as industrial waste.
JP 2002-129248 A (FIG. 1)

しかし、このようなショット粕の埋め立て処分は、資源の有効利用という観点から好ましくない。また、環境悪化を引き起こすとともに、廃棄コストが高くつくという問題もある。
この発明は、前記問題点に鑑みてなされたものであり、ショット粕を有効に再利用することができる製鋼原料用のブリケット及びその製造方法を提供することを目的とする。
However, such landfill disposal of shot dredging is not preferable from the viewpoint of effective use of resources. There are also problems of causing environmental degradation and high disposal costs.
The present invention has been made in view of the above problems, and an object of the present invention is to provide a briquette for a steelmaking raw material and a method for producing the same, which can effectively reuse shot straw.

前記目的を達成するためのこの発明の製鋼原料用のブリケットは、鉄分と油分とを含む乾燥したブリケットであって、鉄系金属の研削切粉とショット粕とを含む綿状凝集体を、固形化補助剤を用いて固形化してなることを特徴としている。
このように構成された製鋼原料用のブリケットは、乾燥した固形物であるので、運搬、貯蔵等の取り扱いが容易である。また、油分を含有するので、ブリケット中の純鉄が酸化するのが防止される。したがって、研削切粉及びショット粕を高品質の製鋼原料として再利用することができる。
The briquette for steelmaking raw material of the present invention for achieving the above object is a dried briquette containing iron and oil, and a solid agglomerate containing iron metal grinding chips and shot soot is solidified. It is characterized by being solidified using a solubilizing aid.
Since the briquette for steelmaking raw material constituted in this way is a dry solid substance, handling such as transportation and storage is easy. Moreover, since oil is contained, it is prevented that the pure iron in a briquette oxidizes. Therefore, the grinding chips and shot iron can be reused as high-quality steelmaking raw materials.

前記製鋼用のブリケットは、ショット粕を5〜25重量%含んでいるのが好ましく、これにより適度の嵩密度と機械的強度を確保することができる。すなわち、ショット粕が5重量%未満であると、嵩密度が小さくなるので、溶鉱炉の形式によっては、当該溶鉱炉への投入時にブリケットがスムーズに落下しないおそれがある。また、ショット粕が25重量%を超えると、ショット粕が偏在した場合に、ブリケットが当該偏在したショット粕部分から割れ易くなる。   It is preferable that the briquette for steel making contains 5 to 25% by weight of shot wrinkles, thereby ensuring appropriate bulk density and mechanical strength. That is, if the shot soot is less than 5% by weight, the bulk density becomes small, and depending on the type of the blast furnace, there is a possibility that the briquette does not fall smoothly when it is put into the blast furnace. If the shot wrinkle exceeds 25% by weight, when the shot wrinkles are unevenly distributed, the briquettes easily break from the unevenly distributed shot wrinkles.

前記ショット粕としては鋼製のショット玉であるのが好ましく、この場合には酸化鉄の含有量が少ないので、製鋼用の原料としてさらに好適なものになる。すなわち、ショット粕は一般に鋼製のショット玉と粉体とを含んでおり、前記ショット玉は純鉄を90重量%以上含み、粉体は酸化した鉄粉を60〜65重量%含んでいる。したがって、ブリケット中の前記粉体の含有量が多いほど、酸化鉄の含有量が多くなる。このため、製鋼時に還元剤の使用量を増やす必要があり、その分、コスト的に不利となるが、ショット粕として前記粉体を除去したショット玉を用いると、ブリケット中の酸化鉄の含有量が少なくなるので、その分、還元剤の使用量を少なくすることができる。   The shot trough is preferably a steel shot ball. In this case, since the iron oxide content is low, it is more suitable as a raw material for steelmaking. That is, the shot basket generally contains steel shot balls and powder, the shot balls contain 90% by weight or more of pure iron, and the powder contains 60 to 65% by weight of oxidized iron powder. Therefore, the higher the content of the powder in the briquette, the higher the content of iron oxide. For this reason, it is necessary to increase the amount of reducing agent used during steelmaking, which is disadvantageous in terms of cost, but if shot balls from which the powder is removed are used as shot troughs, the content of iron oxide in briquettes Therefore, the amount of reducing agent used can be reduced accordingly.

また、この発明の製鋼原料用のブリケットの製造方法は、鉄系金属の研削切粉と油分及び水分を含有する研削液とを含む研削スラッジに、ショット粕を混合して綿状凝集体を得る工程と、前記綿状凝集体を圧縮成形して、繊維状の研削切粉がせん断され且つ余剰の水分及び油分が除去された所定形状の脆性成形体を得る工程と、前記脆性成形体に固形化補助剤を含浸させる工程と、固形化補助剤を含浸させた前記脆性成形体を乾燥させる工程とをこの順に含むことを特徴としている。   In addition, the method for producing briquettes for steelmaking raw materials of the present invention obtains a flocculent aggregate by mixing shot sludge with grinding sludge containing ferrous metal grinding chips and a grinding fluid containing oil and moisture. A step of compression-molding the flocculent aggregate to obtain a brittle molded body having a predetermined shape in which fibrous grinding chips are sheared and excess water and oil are removed; and the brittle molded body is solidified. It comprises a step of impregnating the solubilizing aid and a step of drying the brittle shaped body impregnated with the solidifying aid in this order.

前記の構成の製鋼原料用のブリケットの製造方法によれば、前記綿状凝集体の圧縮成形によって、従来せん断が困難であった繊維状の研削切粉を粗せん断して、ショット粕とともに容易に固形化することができる。また、脆性成形体に含浸させた固形化補助剤によって、当該脆性成形体を圧縮成形するだけで所望の強度に固形化することができるので、綿状凝集体を固形化するために、これを細かく粉砕する必要がない。   According to the manufacturing method of briquettes for steelmaking raw materials having the above-described configuration, the fibrous grinding chips that have been difficult to shear conventionally are roughly sheared by compression molding of the flocculent aggregate, and can be easily performed together with shot iron. It can be solidified. Further, the solidification aid impregnated in the brittle shaped body can be solidified to a desired strength simply by compression molding the brittle shaped body. There is no need to grind finely.

前記ブリケットの製造方法においては、前記ショット粕を10〜30重量%混合するのが好ましい。綿状凝集体中のショット粕が10重量%未満であると、嵩密度の大きいブリケットを得難くなる。また、綿状凝集体中のショット粕が30重量%を超えると、これを固形化し難くなるとともに、ショット粕が偏在した場合に、ブリケットが当該偏在したショット粕部分から割れ易くなる。   In the manufacturing method of the briquette, it is preferable to mix 10 to 30% by weight of the shot basket. If the shot wrinkle in the flocculent aggregate is less than 10% by weight, it is difficult to obtain briquettes having a large bulk density. Further, when the shot wrinkle in the cotton-like aggregate exceeds 30% by weight, it becomes difficult to solidify this, and when the shot wrinkles are unevenly distributed, the briquettes are easily broken from the unevenly distributed shot wrinkles.

前記ショット粕としては鋼製のショット玉を用いるのが好ましく、この場合には、酸化鉄の含有量が少なくなるので、製鋼用の原料としてさらに好適なブリケットを得ることができる。   It is preferable to use steel shot balls as the shot trough. In this case, since the content of iron oxide is reduced, a briquette more suitable as a raw material for steelmaking can be obtained.

前記固形化補助剤としては、珪酸ソーダ、コロイダルシリカ、燐酸アルミニウム、アスファルト乳剤から選択される少なくとも1を用いるのが好ましい。これにより、油分を含む脆性成形体を容易且つ強固に固形化することができる。   As the solidification aid, it is preferable to use at least one selected from sodium silicate, colloidal silica, aluminum phosphate, and asphalt emulsion. Thereby, the brittle molded object containing an oil component can be solidified easily and firmly.

この発明の製鋼原料用のブリケットによれば、研削切粉及びショット粕を高品質の製鋼原料として再利用が可能であり、環境保全に役立つとともに、これら研削切粉及びショット粕の廃棄コストを削減することができる。
また、この発明の製鋼原料用のブリケットの製造方法によれば、脆性成形体に含浸させた固形化補助剤によって、綿状凝集体を細かく粉砕することなく当該脆性成形体を圧縮成形するだけで所望の強度に固形化することができるので、製鋼原料用のブリケットを容易且つ安価に製造することができる。
According to the briquette for steelmaking raw material of the present invention, it is possible to reuse the grinding chips and shot iron as a high-quality steelmaking raw material, which is useful for environmental conservation and reduces the disposal cost of these grinding chips and shot iron. can do.
In addition, according to the method for producing briquettes for steelmaking raw materials of the present invention, the brittle molded body can be simply compression molded without finely pulverizing the flocculent aggregate with the solidification aid impregnated in the brittle molded body. Since it can solidify to desired intensity | strength, the briquette for steelmaking raw materials can be manufactured easily and cheaply.

以下、この発明の実施の形態について添付図面を参照しながら詳述する。
図1はこの発明の一実施形態に係る製鋼原料用のブリケットの製造方法を示す工程図である。このブリケットAの製造においては、まず鉄系金属を研削加工した際に発生する研削スラッジB(図1(a)参照)を、ベルトコンベア1にて搬送しながら、当該研削スラッジBに対してショット粕Sを降りかけて綿状凝集体Mを得る(図1(b)参照)。前記研削スラッジBは研削切粉と研削液とを含む綿状のものである。また、ショット粕Sは鉄系金属にショットブラスを施した際に生じるものであり、ショットによって所定の粒径以下に痩せた使用済みのショット玉と、酸化した鉄粉を60〜65重量%含む粉体とからなるものである。このショット粕Sの混合量は10〜30重量%である。綿状凝集体M中のショット粕Sが10重量%未満であると、嵩密度の大きいブリケットAを得難くなる。また、綿状凝集体M中のショット粕Sが30重量%を超えると、後工程で固形化し難くなるとともに、ショット粕Sが偏在した場合に、ブリケットAが当該偏在したショットS部分から割れ易くなる。
Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings.
FIG. 1 is a process diagram showing a method for producing briquettes for steelmaking raw materials according to one embodiment of the present invention. In manufacturing the briquette A, first, grinding sludge B (see FIG. 1A) generated when iron-based metal is ground is shot on the grinding sludge B while being conveyed by the belt conveyor 1. The cocoon S is lowered to obtain a flocculent aggregate M (see FIG. 1 (b)). The grinding sludge B is a cotton-like one containing grinding chips and grinding fluid. Further, the shot cage S is generated when shot brass is applied to an iron-based metal, and includes a used shot ball thinned to a predetermined particle size or less by shot and 60 to 65% by weight of oxidized iron powder. It consists of powder. The mixing amount of the shot basket S is 10 to 30% by weight. When the shot wrinkle S in the cotton-like aggregate M is less than 10% by weight, it is difficult to obtain the briquette A having a large bulk density. Further, if the shot basket S in the cotton-like aggregate M exceeds 30% by weight, it becomes difficult to solidify in a subsequent process, and when the shot basket S is unevenly distributed, the briquette A is easily broken from the unevenly distributed shot S portion. Become.

次に、前記綿状凝集体Mを加圧圧縮して、研削スラッジBに含まれる研削液の成分である水分及び油分の含有量を予備的に調整する。この綿状凝集体Mの加圧圧縮は、例えば前記ベルトコンベア1の搬送端付近に設けた一対のロール2間に挟み込むことにより行う(図1(b)参照)。この際、綿状凝集体Mは、含水率が50重量%を超えない範囲に、含油率が10重量%を超えない範囲にそれぞれ調整するのが好ましく、これにより、綿状凝集体Mの搬送、貯蔵等の取り扱いが容易となる。   Next, the cotton-like aggregate M is pressurized and compressed to preliminarily adjust the contents of water and oil, which are components of the grinding fluid contained in the grinding sludge B. The pressure-compression of the cotton-like aggregate M is performed, for example, by being sandwiched between a pair of rolls 2 provided near the conveyance end of the belt conveyor 1 (see FIG. 1B). At this time, the flocculent aggregate M is preferably adjusted so that the water content does not exceed 50% by weight and the oil content does not exceed 10% by weight. Handling such as storage becomes easy.

さらに、水分及び油分の含有量が調整された前記綿状凝集体Mを、成形型3を用いてプレスにより圧縮成形して脆性成形体Cを得る(図1(c)参照)。この圧縮成形によって、研削スラッジBに含まれるスパイラル繊維状の研削切粉が粗せん断される。また、余剰の水分及び油分が除去されて、前記脆性成形体Cの含水率が2〜12重量%に、含油率が1〜5重量%に調整される。これにより、最小限の残留油分によって研削切粉が酸化するのを効果的に防止することができる。また、前工程において研削スラッジBの含水率が50重量%、含油率が10重量%をそれぞれ超えない範囲に予め調整されているので、前記脆性成形体Cの水分及び油分の含有割合を圧縮成形のみによって容易かつ適正に調整することができる。
前記脆性成形体Cは、円柱形、球形、角柱形等の取り扱いの容易な形状に形成されているとともに、次工程への搬送時等に崩壊しない程度の強度に固められている。
Further, the flocculent aggregate M in which the moisture and oil contents are adjusted is compression-molded by a press using the mold 3 to obtain a brittle molded body C (see FIG. 1 (c)). By this compression molding, the spiral fibrous grinding chips contained in the grinding sludge B are roughly sheared. Further, excess water and oil are removed, and the moisture content of the brittle shaped body C is adjusted to 2 to 12% by weight and the oil content is adjusted to 1 to 5% by weight. Thereby, it is possible to effectively prevent the grinding chips from being oxidized by the minimum residual oil. In addition, since the water content of the grinding sludge B is adjusted in advance in a range not exceeding 50% by weight and the oil content not exceeding 10% by weight in the previous process, the moisture and oil content ratios of the brittle molded body C are compression molded. It can be adjusted easily and appropriately only by this.
The brittle molded body C is formed in a shape that is easy to handle, such as a cylindrical shape, a spherical shape, and a prismatic shape, and is hardened to such an extent that it does not collapse during transportation to the next process.

次いで、前記脆性成形体Cに、液状の固形化補助剤Dを含浸させる。この固形化補助剤Dの含浸は、例えば脆性成形体Cをベルトコンベア7にて搬送しながら、タンク8に注入した前記固形化補助剤Dに浸漬させることにより行う(図1(d)参照)。この固形化補助剤Dとしては、珪酸ソーダ、コロイダルシリカ、燐酸アルミニウムから選択される少なくとも1種を用いるのが好ましい。この実施の形態においては、主として珪酸ソーダを用いている。この固形化補助剤Dは2〜30重量%含浸させるのが好ましい。これにより、脆性成形体Cを容易且つ強固に固形化することができる。なお、前記固形化補助剤Dとしては、酢酸ビニル等の有機バインダを用いることもできる。   Next, the brittle shaped body C is impregnated with a liquid solidification aid D. The impregnation of the solidification auxiliary D is performed, for example, by immersing the brittle molded body C in the solidification auxiliary D injected into the tank 8 while being conveyed by the belt conveyor 7 (see FIG. 1 (d)). . As the solidification aid D, it is preferable to use at least one selected from sodium silicate, colloidal silica, and aluminum phosphate. In this embodiment, sodium silicate is mainly used. This solidifying auxiliary D is preferably impregnated in an amount of 2 to 30% by weight. Thereby, the brittle molded object C can be solidified easily and firmly. In addition, as said solidification adjuvant D, organic binders, such as vinyl acetate, can also be used.

次に、前記固形化補助剤Dを含浸させた脆性成形体Cを(図1(e)参照)養生(乾燥)してその含有水分を除去することにより(図1(f)参照)、製鋼原料用のブリケットAを得る(図1(g)参照)。この養生は2日間程度行うのが含有水分を確実に除去することができるので好ましい。前記養生に際しては、常温又は冷却されたエアーを吹き付けてこれを急速冷却してもよい。このようにして得られたブリケットAは、ショット粕Sを5〜25重量%含んでいる。   Next, the brittle molded body C impregnated with the solidification aid D is cured (see FIG. 1 (e)) and dried to remove the contained water (see FIG. 1 (f)). Briquette A for raw material is obtained (see FIG. 1 (g)). This curing is preferably performed for about 2 days because the contained water can be removed reliably. In the curing, normal temperature or cooled air may be blown to rapidly cool the air. The briquette A thus obtained contains 5 to 25% by weight of the shot basket S.

前記ブリケットAの形状としては、上述の円柱形状等のほか、卵形、アーモンド形、ラグビーボール形等のような、周縁部に丸みを有し、周縁部から中央部に向かって肉厚が漸次厚くなるほぼピロー形状であってもよい(図2参照)。このような形状に成形することにより、圧縮荷重に強く崩壊し難いとともに、角部等における部分的な破損が生じ難いブリケットAを得ることができる。   As the shape of the briquette A, in addition to the above-described columnar shape, etc., the peripheral portion has a round shape such as an oval shape, an almond shape, a rugby ball shape, and the thickness gradually increases from the peripheral portion toward the central portion. It may have a substantially pillow shape (see FIG. 2). By molding into such a shape, it is possible to obtain a briquette A that is not easily disintegrated strongly against a compressive load and that is difficult to cause partial breakage at corners or the like.

以上により得られたブリケットAは、脆性成形体Cを固形化した多孔質のものであるので、養生によって含有水分を容易且つ確実に除去することができる。このため、そのまま溶鉱炉に投入しても突沸が生じたり舞い上がって排出されたりするおそれがない。
また、ブリケットA中のショット粕Sの含有量が5〜25重量%であるので、適度の嵩密度と機械的強度を有するものとなる。すなわち、製鋼原料用のブリケットAについては、溶鉱炉への投入時に舞い上がることなくスムーズに落下することが要求される。このため、溶鉱炉の種類によっては、嵩密度として0.2以上要求される場合があるが、ブリケットA中のショット粕が5重量%未満であると、この要求を満足し得ないおそれがある。また、ブリケットA中のショット粕が25重量%を超えると、ブリケットA中にショット粕が偏在した場合に、当該ブリケットAがショット粕部分から割れ易くなる。
Since the briquette A obtained as described above is a porous material obtained by solidifying the brittle molded body C, the contained water can be easily and reliably removed by curing. For this reason, there is no possibility that bumping will occur or it will rise and be discharged even if it is put into the blast furnace as it is.
Moreover, since the content of the shot soot S in the briquette A is 5 to 25% by weight, it has an appropriate bulk density and mechanical strength. That is, the briquette A for the steelmaking raw material is required to drop smoothly without being raised at the time of charging into the blast furnace. For this reason, depending on the type of blast furnace, 0.2 or more may be required as a bulk density, but if the shot soot in Briquette A is less than 5% by weight, this requirement may not be satisfied. Further, when the shot wrinkle in the briquette A exceeds 25% by weight, when the shot wrinkle is unevenly distributed in the briquette A, the briquette A is easily broken from the shot wrinkle portion.

さらに、前記ブリケットAの製造方法においては、研削液の油分の一部を常に保持した状態で加工しているので、純鉄の酸化が効果的に防止されている。例えば軸受鋼(SUJ−2)の研削切粉を含む研削スラッジBを用いて製造されたブリケットAについては、60〜90重量%の純鉄を含むことが確認されている。したがって、溶解歩留まりが80%以上と非常に高く、高品質の製鋼原料として製鋼メーカに有償で提供することができる。しかも、固形にて運搬その他の取り扱いが容易である。
しかも、前記製造方法は、綿状凝集体Mを粉砕して微細化する工程を要することなく当該綿状凝集体Mを固形化することができるので、ブリケットAを能率よく製造することができる。
Furthermore, in the manufacturing method of the briquette A, since processing is performed in a state in which a part of the oil of the grinding fluid is always held, oxidation of pure iron is effectively prevented. For example, it has been confirmed that briquette A manufactured using grinding sludge B containing grinding chips of bearing steel (SUJ-2) contains 60 to 90% by weight of pure iron. Therefore, the melting yield is as high as 80% or more, and can be provided to steel makers as a high-quality steelmaking raw material for a fee. In addition, it is easy to transport and handle in solid form.
And since the said manufacturing method can solidify the said cotton-like aggregate M, without requiring the process which grind | pulverizes and refines | miniaturizes the cotton-like aggregate M, the briquette A can be manufactured efficiently.

前記したブリケットAの製造方法は、炭素を0.2重量%以上含む研削切粉を再利用するのに特に好適に適用される。このような研削切粉は、スプリングバックが大きく、固形化が困難であるが、この発明の製造方法を適用することにより、当該スプリングバックの影響を排除して強固に固形化されたブリケットAを容易に得ることができる。なお、炭素を0.2重量%以上含む研削切粉の代表例としては、軸受鋼の研削切粉を挙げることができる。   The above-described method for producing briquette A is particularly suitably applied to reuse grinding chips containing 0.2 wt% or more of carbon. Such grinding chips have a large spring back and are difficult to solidify. By applying the manufacturing method of the present invention, the briquette A solidified by eliminating the influence of the spring back can be obtained. Can be easily obtained. In addition, as a representative example of the grinding chips containing 0.2 wt% or more of carbon, there can be mentioned grinding chips of bearing steel.

前記実施の形態においては、ショット粕Sとして使用済のショット玉と、酸化した鉄粉を含む粉体とを有するものを用いたが、前記粉体を選別除去してショット玉のみとしたものを用いてもよい。この場合には、ブリケットA中の酸化鉄の含有量が少なくなるので、その分、製鋼時に還元剤の使用量を少なくすることができる。このため、製鋼原料用の原料としてさらに好適なものになる。   In the above-described embodiment, the shot basket S having a used shot ball and a powder containing oxidized iron powder is used, but only the shot ball is obtained by selectively removing the powder. It may be used. In this case, since the content of iron oxide in the briquette A is reduced, it is possible to reduce the amount of reducing agent used during steel making. For this reason, it becomes a more suitable thing as a raw material for steelmaking raw materials.

この発明の一実施形態に係る製鋼原料用のブリケットの製造方法を示す工程図である。It is process drawing which shows the manufacturing method of the briquette for the steelmaking raw materials which concerns on one Embodiment of this invention. ブリケットの一部欠截斜視図である。It is a partial missing perspective view of a briquette.

符号の説明Explanation of symbols

A ブリケット
B 研削スラッジ
C 脆性成形体
D 固形化補助剤
M 綿状凝集体
S ショット粕
A Briquette B Grinding sludge C Brittle shaped body D Solidification aid M Cotton-like aggregate S Shot glaze

Claims (7)

鉄分と油分とを含む乾燥したブリケットであって、鉄系金属の研削切粉とショット粕とを含む綿状凝集体を、固形化補助剤を用いて固形化してなることを特徴とする製鋼原料用のブリケット。   A dry briquette containing iron and oil, which is obtained by solidifying a flocculent agglomerate containing iron-based metal grinding chips and shot straw using a solidification aid. Briquette. 前記ショット粕を5〜25重量%含む請求項1記載の製鋼原料用のブリケット。   The briquette for steelmaking raw materials of Claim 1 containing 5-25 weight% of said shot straws. 前記ショット粕が、鋼製のショット玉である請求項1記載の製鋼原料用のブリケット。   The briquette for a steelmaking raw material according to claim 1, wherein the shot trough is a steel shot ball. 鉄系金属の研削切粉と油分及び水分を含有する研削液とを含む研削スラッジに、ショット粕を混合して綿状凝集体を得る工程と、
前記綿状凝集体を圧縮成形して、繊維状の研削切粉がせん断され且つ余剰の水分及び油分が除去された所定形状の脆性成形体を得る工程と、
前記脆性成形体に固形化補助剤を含浸させる工程と、
固形化補助剤を含浸させた前記脆性成形体を乾燥させる工程と
をこの順に含むことを特徴とする製鋼原料用のブリケットの製造方法。
A step of mixing a cotton cake with a grinding sludge containing a ferrous metal grinding chip and a grinding fluid containing oil and moisture to obtain a flocculent aggregate,
A step of compression-molding the cotton-like aggregate to obtain a brittle molded body having a predetermined shape in which fibrous grinding chips are sheared and excess water and oil are removed;
Impregnating the brittle shaped body with a solidification aid;
And a step of drying the brittle shaped body impregnated with the solidification aid in this order.
前記ショット粕を10〜30重量%混合する請求項4記載の製鋼原料用のブリケットの製造方法。   The manufacturing method of the briquette for the steelmaking raw materials of Claim 4 which mixes 10-30 weight% of said shot straws. 前記ショット粕が鋼製のショット玉である請求項4記載の製鋼原料用のブリケットの製造方法。   The method for producing briquettes for a steelmaking raw material according to claim 4, wherein the shot trough is a steel shot ball. 前記固形化補助剤が、珪酸ソーダ、コロイダルシリカ、燐酸アルミニウム、アスファルト乳剤から選択される少なくとも1種である請求項4記載の製鋼原料用のブリケットの製造方法。   The method for producing briquettes for a steelmaking raw material according to claim 4, wherein the solidification aid is at least one selected from sodium silicate, colloidal silica, aluminum phosphate, and asphalt emulsion.
JP2004050197A 2004-02-25 2004-02-25 Briquette for raw material for steelmaking and method for manufacturing the same Pending JP2005240087A (en)