JP2002356660A - Double-coated adhesive tape and bonded product - Google Patents

Double-coated adhesive tape and bonded product

Info

Publication number
JP2002356660A
JP2002356660A JP2001227833A JP2001227833A JP2002356660A JP 2002356660 A JP2002356660 A JP 2002356660A JP 2001227833 A JP2001227833 A JP 2001227833A JP 2001227833 A JP2001227833 A JP 2001227833A JP 2002356660 A JP2002356660 A JP 2002356660A
Authority
JP
Japan
Prior art keywords
double
adhesive tape
sensitive adhesive
pressure
nonwoven fabric
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP2001227833A
Other languages
Japanese (ja)
Inventor
Kazuyuki Fukuyama
和行 福山
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Sekisui Chemical Co Ltd
Original Assignee
Sekisui Chemical Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sekisui Chemical Co Ltd filed Critical Sekisui Chemical Co Ltd
Priority to JP2001227833A priority Critical patent/JP2002356660A/en
Publication of JP2002356660A publication Critical patent/JP2002356660A/en
Pending legal-status Critical Current

Abstract

PROBLEM TO BE SOLVED: To provide a double-coated adhesive tape which is excellent in strength against delamination from an adhered matter and adaptability to a complicated shape, and a float or a peeling-free bonded product using the double-coated adhesive tape. SOLUTION: The double-coated adhesive tape comprises an adhesive layer laminated over the both sides of a curved surface-adaptable nonwoven fabric, wherein the nonwoven fabric has a longitudinal elongation and a lateral strain of 100% or more and an stress of 3 N/cm or less at 100% strain. The bonded product can be produced by bonding a polyolefine material by the double-coated adhesive tape.

Description

【発明の詳細な説明】DETAILED DESCRIPTION OF THE INVENTION

【0001】[0001]

【発明の属する技術分野】本発明は内装材等の接合に好
適に用いられる両面粘着テープ、及び、両面テープを用
いて接合されてなる接合体に関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a double-sided pressure-sensitive adhesive tape suitably used for bonding interior materials and the like, and a bonded body bonded using the double-sided tape.

【0002】[0002]

【従来の技術】環境保護の一環として、近年、脱塩化ビ
ニル樹脂・リサイクル化の中で環境に優しいプラスチッ
クの需要が急増している。このような社会環境下で、特
に自動車部品、家電製品、包装材などの分野では樹脂部
材のオレフィン化が急速に進んできている。しかしなが
ら、一般に無極性樹脂であるオレフィン樹脂は難被着体
であるので、オレフィン樹脂系部材同士の接合を行う際
は、比較的極性の高い汎用のアクリル樹脂系粘着剤によ
る接合は困難とされてきた。そのため、オレフィン樹脂
系部材の接合方法としては、嵌合・ネジ止め・融着・ホ
ットメルト接着剤などによる接合が一般的となってい
た。
2. Description of the Related Art In recent years, as part of environmental protection, demand for environmentally friendly plastics has been rapidly increasing in the course of recycling vinyl chloride resin. Under such a social environment, olefination of resin members is rapidly progressing particularly in the fields of automobile parts, home electric appliances, packaging materials and the like. However, since an olefin resin, which is a nonpolar resin, is generally a difficult adherend, it has been considered difficult to join olefin resin-based members with a general-purpose acrylic resin-based pressure-sensitive adhesive having a relatively high polarity. Was. Therefore, as a method of joining olefin resin-based members, fitting, screwing, fusion, hot-melt adhesive, and the like have been common.

【0003】しかし、上記接合方法は、接合に時間がか
かる、品質がばらつくなどの潜在的な問題があった。こ
のような問題を解決するために、例えば、特開平08−
27440号公報に記載のように、不織布基材に粘着層
を設けた粘着テープを使用する方法が、簡便性の点で従
来の主流となっていた。
[0003] However, the above-mentioned joining method has potential problems such as a long joining time and a variation in quality. In order to solve such a problem, for example, Japanese Patent Application Laid-Open
As described in Japanese Patent No. 27440, a method using an adhesive tape provided with an adhesive layer on a nonwoven fabric substrate has been the mainstream of the conventional method in terms of simplicity.

【0004】[0004]

【発明が解決しようとする課題】しかしながら本発明者
の検討によれば、上記のような不織布を基材とする粘着
テープは、接合体に何らかの応力が働いた場合に、剥離
応力が被着体と粘着剤との界面に集中するため、割裂剥
離等が発生することがあり、剥離強度が必ずしも充分で
はなかった。また、一般に、不織布を基材とする粘着テ
ープは、凹凸への追従性に劣るため、乗り物用内装材の
ような曲面を有する複雑形状の被着体に用いた場合に、
接合部に浮きや剥がれが発生しやすいといった欠点があ
った。
However, according to the study of the present inventor, the pressure-sensitive adhesive tape based on the nonwoven fabric as described above shows that when a certain stress acts on the joined body, the peeling stress is increased on the adherend. Since it is concentrated on the interface between the adhesive and the adhesive, split peeling or the like may occur, and the peel strength is not always sufficient. In addition, in general, an adhesive tape based on a nonwoven fabric is inferior in conformity to irregularities, so when used for an adherend of a complicated shape having a curved surface such as a vehicle interior material,
There was a drawback that the joint was likely to float or peel off.

【0005】本発明者の得た上記知見に鑑み、本発明の
目的は、被着体からの剥離強度に優れ、複雑形状への追
従性に優れた両面粘着テープを提供すると共に、両面粘
着テープを用いた浮きや剥がれの発生しにくい接合体を
提供することにある。なお、本発明における両面粘着テ
ープには両面粘着シートも含まれるものとする。
In view of the above findings obtained by the present inventors, an object of the present invention is to provide a double-sided pressure-sensitive adhesive tape having excellent peel strength from an adherend and excellent conformability to a complicated shape. An object of the present invention is to provide a joined body that is less likely to be lifted or peeled off. The double-sided pressure-sensitive adhesive tape of the present invention includes a double-sided pressure-sensitive adhesive sheet.

【0006】[0006]

【課題を解決するための手段】上記目的を達成するため
に、請求項1記載の発明は、曲面追従性を有する不織布
の両面に粘着層が設けられてなる両面粘着テープを提供
する。又、請求項2記載の発明は、不織布が、縦及び横
方向の伸度が各100%以上であり、100%伸長強度
が3N/cm以下である請求項1記載の両面粘着テープ
を提供する。
In order to achieve the above object, the invention according to claim 1 provides a double-sided pressure-sensitive adhesive tape comprising a nonwoven fabric having curved surface followability, and pressure-sensitive adhesive layers provided on both sides. The invention according to claim 2 provides the double-sided pressure-sensitive adhesive tape according to claim 1, wherein the nonwoven fabric has an elongation in the longitudinal and lateral directions of 100% or more, respectively, and a 100% elongation strength of 3 N / cm or less. .

【0007】又、請求項3記載の発明は、粘着層が、炭
素数4〜10のアルキル基を有するアルキル(メタ)ア
クリレートが30〜95重量%の割合で含有され共重合
されてなるアクリル系共重合体を主成分とするアクリル
系粘着剤からなる、請求項1又は2記載の両面粘着テー
プを提供する。又、請求項4記載の発明は、請求項1〜
3の何れか1項記載の両面粘着テープを用いてポリオレ
フィン系部材が接合されてなる接合体を提供する。
[0007] The invention according to claim 3 is an acrylic system wherein the pressure-sensitive adhesive layer is copolymerized by containing an alkyl (meth) acrylate having an alkyl group having 4 to 10 carbon atoms in a proportion of 30 to 95% by weight. The double-sided pressure-sensitive adhesive tape according to claim 1, comprising an acrylic pressure-sensitive adhesive containing a copolymer as a main component. Further, the invention described in claim 4 is based on claims 1 to
3. A joined body formed by joining a polyolefin-based member using the double-sided pressure-sensitive adhesive tape according to any one of 3.

【0008】以下、本発明について更に詳しく説明す
る。本発明に用いられる不織布としては、曲面追従性を
有するものであれば特に限定されず、例えば、厚さ50
0μm以下のウレタン樹脂系不織布、ポリオレフィン樹
脂系不織布、ポリエステル樹脂系不織布等が挙げられ
る。なかでも、不織布の縦及び横方向の伸度が各100
%以上のものが好ましく、また、その100%伸長強度
が各3N/cm以下のものが好ましい。
Hereinafter, the present invention will be described in more detail. The nonwoven fabric used in the present invention is not particularly limited as long as it has a curved surface following property.
A urethane resin-based nonwoven fabric having a thickness of 0 μm or less, a polyolefin resin-based nonwoven fabric, a polyester resin-based nonwoven fabric, and the like can be given. In particular, the elongation of the nonwoven fabric in the vertical and horizontal directions is 100
% Or more, and those having a 100% elongation strength of 3 N / cm or less.

【0009】上記伸度が100%に満たない場合は、乗
り物用内装材のような複雑形状の成形品に、ポリエチレ
ン樹脂系の発泡シート等の部材を、環状や非線形に貼付
した場合、部材の曲げ部の内側にしわ等が入りやすくな
る。また、上記100%伸長強度が各3N/cmを越え
ると貼付け時の引張応力で剥がれることがある。伸度の
上限及び100%伸長強度の下限は特に認められない
が、伸度が高くなり過ぎると不用意に伸びて貼付作業の
作業性が悪くなりやすく、また、100%伸長強度が低
くなりすぎると曲面等に貼付する際の追従性が悪いので
注意を要する。
When the elongation is less than 100%, when a member such as a polyethylene resin foam sheet is attached to a molded article having a complicated shape such as an interior material for a vehicle in a circular or non-linear manner, Wrinkles and the like easily enter the inside of the bent portion. Further, if the 100% elongation exceeds 3 N / cm, peeling may occur due to tensile stress at the time of sticking. The upper limit of the elongation and the lower limit of the 100% elongation are not particularly recognized. However, if the elongation is too high, the workability of the sticking work is liable to be deteriorated easily, and the 100% elongation is too low. Care must be taken because the follow-up property when sticking to curved surfaces and the like is poor.

【0010】本発明における粘着層を構成す粘着剤は、
特に限定されず、炭素数4〜10のアルキル基を有する
アルキル(メタ)アクリレートが30〜95重量%の割
合で含有され共重合されてなるアクリル系共重合体を主
成分とするアクリル系粘着剤であることが好ましい。上
記アルキル(メタ)アクリレートの含有量が95重量%
を越える場合は耐熱性に乏しくなり低温時の使用性等が
悪くなる場合がある。
The pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer according to the present invention comprises:
There is no particular limitation, and an acrylic pressure-sensitive adhesive containing, as a main component, an acrylic copolymer obtained by copolymerizing an alkyl (meth) acrylate having an alkyl group having 4 to 10 carbon atoms in a proportion of 30 to 95% by weight. It is preferred that The content of the alkyl (meth) acrylate is 95% by weight.
If the ratio exceeds the above range, the heat resistance may be poor and the usability at low temperatures may be deteriorated.

【0011】上記アルキル(メタ)アクリレートとして
は、例えば、n−ブチルアクリレート、2−エチルヘキ
シル(メタ)アクリレート、イソオクチル(メタ)アク
リレート、n−オクチル(メタ)アクリレート、ノニル
(メタ)アクリレート、デシル(メタ)アクリレート等
のアルキル(メタ)アクリレート等が挙げられこれらは
単独または組み合わせて用いることができる。
Examples of the alkyl (meth) acrylate include n-butyl acrylate, 2-ethylhexyl (meth) acrylate, isooctyl (meth) acrylate, n-octyl (meth) acrylate, nonyl (meth) acrylate, and decyl (meth) acrylate. ) Alkyl (meth) acrylates such as acrylate and the like, and these can be used alone or in combination.

【0012】上記アクリル系共重合体には、ポリオレフ
ィンへの接着性を上げるために、末端に重合性不飽和二
重結合を有するオレフィン系重合体を共重合させたもの
であってもよい。上記重合性不飽和二重結合を有するオ
レフィン系重合体としては、他のビニルモノマーと共重
合可能な二重結合とオレフィン骨格とからなるポリマー
構造を有するものであれば特に限定されず、上記オレフ
ィン骨格としては、例えばエチレン−ブチレンランダム
共重合体、エチレン−プロピレン共重合体等が挙げられ
る。
The above-mentioned acrylic copolymer may be obtained by copolymerizing an olefin polymer having a polymerizable unsaturated double bond at a terminal in order to increase the adhesion to polyolefin. The olefin polymer having a polymerizable unsaturated double bond is not particularly limited as long as it has a polymer structure comprising a double bond copolymerizable with another vinyl monomer and an olefin skeleton. Examples of the skeleton include an ethylene-butylene random copolymer and an ethylene-propylene copolymer.

【0013】上記アクリル系共重合体は、従来公知の重
合方法で製造され得る。例えば、溶媒中で溶液重合され
たものであってもよいし、また塊状重合されたものであ
ってもよい。塊状重合法としては、工業的生産上、溶媒
としての有機溶剤や水分を乾燥する必要がない光重合法
が好適である。紫外線を照射する光重合法によって得ら
れたアクリル系共重合体は分子量の再現性も良く、従っ
て、この共重合体を主成分とするアクリル系粘着剤の物
性も良好なものが得られる。
The acrylic copolymer can be produced by a conventionally known polymerization method. For example, it may be solution-polymerized in a solvent or may be bulk-polymerized. As the bulk polymerization method, a photopolymerization method that does not require drying of an organic solvent or water as a solvent in industrial production is suitable. The acrylic copolymer obtained by the photopolymerization method of irradiating ultraviolet rays has a good reproducibility of the molecular weight, and therefore, an acrylic pressure-sensitive adhesive containing this copolymer as a main component has good physical properties.

【0014】本発明におけるアクリル系粘着剤は、上記
アクリル共重合体を主成分とし、耐熱性やクリープ性を
向上させるために、従来公知の架橋剤が添加配合された
ものであるのが好ましい。架橋剤として、例えば、イソ
シアネート系、エポキシ系、アジリジン系の架橋剤が多
用される。また、このような架橋剤と確実に架橋反応が
進行するように、上記アクリル系共重合体には極性基を
有する共重合性モノマーが構成成分として導入されてい
るのが好ましい。
The acrylic pressure-sensitive adhesive of the present invention preferably contains the above-mentioned acrylic copolymer as a main component and is added with a conventionally known crosslinking agent in order to improve heat resistance and creep properties. As the crosslinking agent, for example, an isocyanate-based, epoxy-based, or aziridine-based crosslinking agent is frequently used. Further, it is preferable that a copolymerizable monomer having a polar group is introduced as a component into the acrylic copolymer so that the crosslinking reaction proceeds with such a crosslinking agent without fail.

【0015】このような共重合性モノマーとしては、例
えば、スチレン、α−メチルスチレン、o−メチルスチ
レン、p−メチルスチレン等のスチレン系モノマー:酢
酸ビニルなどのカルボン酸ビニルエステル:アクリル
酸、メタクリル酸等のビニル基含有カルボン酸またはカ
ルボン酸無水物:2−ヒドロキシエチル(メタ)アクリ
レート、4−ヒドロキシブチルアクリレートなどの水酸
基含有ビニルモノマー:(メタ)アクリルニトリル、N
−ビニルピロリドンなどの窒素含有モノマー等が挙げら
れる。なかでも、カルボン酸を有するアクリル酸やメタ
クリル酸、水酸基を有する2−ヒドロキシエチル(メ
タ)アクリレート等がイソシアネート系架橋剤もしくは
エポキシ系架橋剤との反応に由来する架橋構造を形成す
る上でより好適に用いられる。
Examples of such a copolymerizable monomer include styrene-based monomers such as styrene, α-methylstyrene, o-methylstyrene and p-methylstyrene; carboxylic acid vinyl esters such as vinyl acetate: acrylic acid and methacrylic acid. Vinyl group-containing carboxylic acid or carboxylic anhydride such as acid: 2-hydroxyethyl (meth) acrylate, hydroxyl group-containing vinyl monomer such as 4-hydroxybutyl acrylate: (meth) acrylonitrile, N
And nitrogen-containing monomers such as vinylpyrrolidone. Above all, acrylic acid and methacrylic acid having a carboxylic acid, 2-hydroxyethyl (meth) acrylate having a hydroxyl group, and the like are more preferable in forming a crosslinked structure derived from a reaction with an isocyanate-based crosslinking agent or an epoxy-based crosslinking agent. Used for

【0016】又、架橋構造を形成させるために、共重合
可能な不飽和二重結合を分子内に2個以上有するモノマ
ーが共重合されていてもよい。このようなモノマーとし
て、例えば、ヘキサンジオールジ(メタ)アクリレー
ト、(ポリ)エチレングリコールジ(メタ)アクリレー
ト、(ポリ)プロピレングリコールジ(メタ)アクリレ
ート、ウレタンアクリレート、ポリエステルアクリレー
ト等が挙げられる。
Further, in order to form a crosslinked structure, a monomer having two or more copolymerizable unsaturated double bonds in a molecule may be copolymerized. Examples of such a monomer include hexanediol di (meth) acrylate, (poly) ethylene glycol di (meth) acrylate, (poly) propylene glycol di (meth) acrylate, urethane acrylate, and polyester acrylate.

【0017】本発明におけるアクリル系粘着剤は、上記
アクリル共重合体を主成分とし、必要に応じて、更に、
粘着付与剤、可塑剤、軟化剤、無機及び有機充填剤、顔
料、染料等が適宜配合されて用いられる。上記粘着付与
剤としては特に限定されず、従来公知の、ロジン系樹
脂、変性ロジン系樹脂、テルペン系樹脂、テルペンフェ
ノール系樹脂、C5及びC9系石油樹脂やこれらの水添
物等が挙げられる。また、これらは単独又は2種以上組
み合わせて用いることができる。
The acrylic pressure-sensitive adhesive of the present invention contains the above-mentioned acrylic copolymer as a main component, and if necessary, further comprises
Tackifiers, plasticizers, softeners, inorganic and organic fillers, pigments, dyes and the like are appropriately blended and used. The tackifier is not particularly limited, and includes conventionally known rosin resins, modified rosin resins, terpene resins, terpene phenol resins, C5 and C9 petroleum resins, and hydrogenated products thereof. These can be used alone or in combination of two or more.

【0018】本発明における粘着層の厚みとしては、特
に限定されないが、40〜1000μmであることが好
ましく、より好ましくは70〜600μmである。40
μmに満たない場合は被着体表面の凹凸に追従しにくく
なり、1000μmを越えると不織布の柔軟性を損なっ
てしまう。
The thickness of the adhesive layer in the present invention is not particularly limited, but is preferably from 40 to 1000 μm, and more preferably from 70 to 600 μm. 40
When it is less than μm, it is difficult to follow irregularities on the surface of the adherend, and when it exceeds 1000 μm, the flexibility of the nonwoven fabric is impaired.

【0019】本発明における両面粘着テープの製造方法
は、特に限定されないが、例えば、一面に粘着層が設け
られた剥離紙を2個用意し、曲面追従性を有する不織布
の一面に一方の剥離紙を重ね合わせて転写により粘着層
を形成し、他方の面にも同様にして粘着層を形成する方
法等により製造される。本発明の接合体はポリオレフィ
ン系部材が接合されてなるものであり、一方がポリオレ
フィン樹脂成型品で他方がポリオレフィン樹脂発泡体で
ある場合が代表的であるが、一方がポリオレフィン樹脂
成型品もしくはポリオレフィン樹脂発泡体であり、他方
が金属やガラス等であってもよい。
The method for producing the double-sided pressure-sensitive adhesive tape of the present invention is not particularly limited. For example, two release papers each having an adhesive layer provided on one surface are prepared, and one release paper is provided on one surface of a nonwoven fabric having a curved surface following property. Are laminated to form an adhesive layer by transfer, and the other surface is similarly formed by a method of forming an adhesive layer. The joined body of the present invention is obtained by joining polyolefin-based members, and one of the joined bodies is typically a polyolefin resin molded article and the other is a polyolefin resin foam, but one is a polyolefin resin molded article or a polyolefin resin. It may be a foam, the other of which may be metal or glass.

【0020】[0020]

【発明の実施の形態】次に、本発明の接合体について、
以下、図面を参照しながら説明する。図1は本発明の接
合体の一例を示す模式図であり、自動車用内装材を表わ
す。本発明の接合体は、請求項1〜3の何れかに記載の
両面粘着テープを用いて接合されたものであり、部材1
と部材2とを本発明の両面粘着テープ3で接合したもの
である。
Next, the joined body of the present invention will be described.
This will be described below with reference to the drawings. FIG. 1 is a schematic view showing one example of the joined body of the present invention, and shows an interior material for an automobile. The joined body of the present invention is joined using the double-sided pressure-sensitive adhesive tape according to any one of claims 1 to 3, and is a member 1
And the member 2 are joined with the double-sided adhesive tape 3 of the present invention.

【0021】部材1は、例えば内装材の表装材として用
いられる、ポリプロピレン樹脂発泡シートであり、緩衝
材としての役割を有するものである。部材2は、予め熱
成形加工されたポリオレフィン樹脂成型品である。本発
明の接合体を製造するには、例えば、ポリオレフィン樹
脂成型品2に両面粘着テープ3の一方の剥離紙を剥ぎ取
って露出した粘着層をコーナー部に沿って貼り付け、他
方の粘着層にポリプロピレン樹脂発泡シート1をのせて
圧着するとよい。
The member 1 is, for example, a foamed polypropylene resin sheet used as a surface covering material of an interior material, and has a role as a cushioning material. The member 2 is a polyolefin resin molded product that has been thermoformed in advance. In order to manufacture the joined body of the present invention, for example, one of the release papers of the double-sided adhesive tape 3 is peeled off from the polyolefin resin molded article 2 and the exposed adhesive layer is attached along the corner portion, and the other adhesive layer is attached to the other adhesive layer. It is advisable to place the polypropylene resin foam sheet 1 and press it on.

【0022】(作用)本発明の両面粘着テープにおいて
は、曲面追従性を有する不織布を用いることにより、複
雑な形状の被着体に追従しやすくなることに加えて、接
合部に剥離力が働いた場合には、被着体と粘着剤との界
面に応力が集中するのを著しく減少させることができる
ため、被着体からの剥離強度を大幅に向上することがで
きる。このため被着体がオレフィン樹脂系部材であって
も、充分な剥離強度を得ることが可能となる。また、不
織布の伸度が100%以上であり100%伸長強度が3
N/cm以下であると上記効果は更に確実なものとな
る。本発明の接合体は、上記のような特徴を有する両面
粘着テープを用いて接合されてなるので、接合界面にお
いて浮きや剥がれが発生しにくい接合体を得ることがで
きる。
(Function) In the double-sided pressure-sensitive adhesive tape of the present invention, by using a nonwoven fabric having a curved surface followability, it is easy to follow an adherend having a complicated shape, and in addition, a peeling force acts on a joint portion. In this case, since the concentration of stress at the interface between the adherend and the pressure-sensitive adhesive can be significantly reduced, the peel strength from the adherend can be greatly improved. For this reason, even if the adherend is an olefin resin-based member, it is possible to obtain a sufficient peel strength. In addition, the elongation of the nonwoven fabric is 100% or more, and the 100% elongation strength is 3%.
When the value is N / cm or less, the above-mentioned effect is further ensured. Since the joined body of the present invention is joined by using the double-sided pressure-sensitive adhesive tape having the above-described characteristics, a joined body in which floating or peeling is less likely to occur at the joining interface can be obtained.

【0023】[0023]

【実施例】以下に実施例および比較例を示すことによ
り、本発明を具体的に説明する。尚、本発明は下記実施
例のみに限定されるものではない。また、「部」とある
のは「重量部」を意味する。 (実施例1)冷却管、温度計及び攪拌機を備えたセパラ
ブルフラスコに、ブチルアクリレート30部、2−エチ
ルヘキシルアクリレート60部及びアクリル酸2部を、
合計量が酢酸エチルに対して重量比で55/45になる
ように酢酸エチルに溶解し、得られた溶液に重合開始剤
としてベンゾイルパーオキサイド0.062部を添加し
た。
EXAMPLES The present invention will be specifically described below with reference to examples and comparative examples. The present invention is not limited only to the following examples. Further, “parts” means “parts by weight”. (Example 1) 30 parts of butyl acrylate, 60 parts of 2-ethylhexyl acrylate and 2 parts of acrylic acid were placed in a separable flask equipped with a cooling tube, a thermometer and a stirrer.
It was dissolved in ethyl acetate so that the total amount was 55/45 by weight with respect to ethyl acetate, and 0.062 part of benzoyl peroxide was added as a polymerization initiator to the obtained solution.

【0024】この混合溶液を窒素還流下、80℃8時間
攪拌して重合を行い、アクリル系共重合体溶液を得て、
更に、架橋剤として、トリレンジイソシアネートトリメ
チロールプロパン変性体(日本ポリウレタン社製、商品
名「コロネートL」)を、アクリル系共重合体100部
に対して2.0部添加配合し、粘着剤組成物を調製し
た。得られた粘着剤組成物を、ナイフコーターにてPE
Tフィルム(厚さ38μm)に乾燥後膜厚75μmとな
るようキャスチングし、ギアオーブンにて105℃で3
分間乾燥を行った後、不織布に両面貼付し、両面粘着テ
ープを得た。なお、不織布としてはウレタン不織布(カ
ネボウ社製、商品名「エスパンシオーネUHO50」、
伸度及び伸長強度は表1に記載)を用いた。
This mixed solution was stirred at 80 ° C. for 8 hours under nitrogen reflux to carry out polymerization to obtain an acrylic copolymer solution.
Further, as a cross-linking agent, 2.0 parts of a modified tolylene diisocyanate trimethylolpropane (trade name "Coronate L" manufactured by Nippon Polyurethane Co., Ltd.) was added to 100 parts of the acrylic copolymer, and the mixture was mixed with an adhesive composition. Was prepared. The obtained pressure-sensitive adhesive composition is PE-coated with a knife coater.
After drying on a T film (thickness: 38 μm), the film is cast to a thickness of 75 μm, and then dried in a gear oven at 105 ° C. for 3 hours.
After drying for 2 minutes, both sides were adhered to a nonwoven fabric to obtain a double-sided adhesive tape. In addition, as the nonwoven fabric, urethane nonwoven fabric (manufactured by Kanebo Co., Ltd., trade name "Espancione UHO50",
The elongation and elongation strength described in Table 1 were used.

【0025】(実施例2)不織布として伸縮性ポリオレ
フィン不織布(出光石油化学社製、商品名「ストラテッ
クAF70E」)を用いたこと以外は、実施例1と同様
の方法にて両面粘着テープを得た。
(Example 2) A double-sided pressure-sensitive adhesive tape was obtained in the same manner as in Example 1 except that a stretchable polyolefin nonwoven fabric (trade name: Stratec AF70E, manufactured by Idemitsu Petrochemical Co., Ltd.) was used as the nonwoven fabric. Was.

【0026】(実施例3)ブチルアクリレート30部、
2−エチルヘキシルアクリレート60部及びアクリル酸
2部を、均一に混合し、光開始剤(チバカイギ社製 商
品名「イルカギュアー651 」)0.1部を配合した後、
紫外線ランプを用いて厚み75μmに塊状重合した後、
不織布に両面貼付し、両面粘着テープを得た。なお、不
織布としては、伸縮性ポリエステル不織布(帝人社製、
商品名「R291」)を用いた。
(Example 3) 30 parts of butyl acrylate
60 parts of 2-ethylhexyl acrylate and 2 parts of acrylic acid were uniformly mixed, and 0.1 part of a photoinitiator (trade name “Ilkaguer 651” manufactured by Ciba Kaigi Co., Ltd.) was added.
After mass polymerization to a thickness of 75 μm using an ultraviolet lamp,
A double-sided adhesive tape was obtained by affixing to both sides of the nonwoven fabric. In addition, as the nonwoven fabric, a stretchable polyester nonwoven fabric (manufactured by Teijin Limited,
The trade name "R291") was used.

【0027】(実施例4)図1に示すように、部材1と
部材2とを、実施例1で得られた両面粘着テープを用い
て接合し接合体を作製した。なお、部材1としては厚み
3mm、20倍発泡の架橋発泡ポリエチレン発泡体を用
い、部材2としては、厚み1.5mmのオレフィン成型
品を用いた。
Example 4 As shown in FIG. 1, a member 1 and a member 2 were joined using the double-sided pressure-sensitive adhesive tape obtained in Example 1 to produce a joined body. As the member 1, a cross-linked foamed polyethylene foam having a thickness of 3 mm and a 20-fold expansion was used, and as the member 2, an olefin molded product having a thickness of 1.5 mm was used.

【0028】(実施例5)実施例2で得られた両面粘着
テープを用いたこと以外は実施例4と同様にして接合体
を作製した。 (実施例6)実施例3で得られた両面粘着テープを用い
たこと以外は実施例4と同様にして接合体を作製した。
Example 5 A joined body was produced in the same manner as in Example 4 except that the double-sided pressure-sensitive adhesive tape obtained in Example 2 was used. (Example 6) A joined body was produced in the same manner as in Example 4 except that the double-sided pressure-sensitive adhesive tape obtained in Example 3 was used.

【0029】(比較例1)不織布としてパルプ系不織布
(日本紙業社製、商品名「SPC14」)を用いたこと
以外は実施例1と同様の方法にて両面粘着テープを得
た。 (比較例2)不織布としてポリエステル不織布(ユニチ
カ社製、商品名「スパンボンド20451FLV」)を
用いたこと以外は、実施例1と同様の方法にて両面粘着
テープを得た。
Comparative Example 1 A double-sided pressure-sensitive adhesive tape was obtained in the same manner as in Example 1, except that a pulp-based nonwoven fabric (trade name "SPC14", manufactured by Nippon Paper Industries) was used as the nonwoven fabric. (Comparative Example 2) A double-sided pressure-sensitive adhesive tape was obtained in the same manner as in Example 1, except that a polyester non-woven fabric (product name: Spunbond 20451 FLV, manufactured by Unitika Ltd.) was used as the non-woven fabric.

【0030】(比較例3)比較例1で得られた両面粘着
テープを用いたこと以外は実施例4と同様にして接合体
を作製した。 (比較例4)比較例2で得られた両面粘着テープを用い
たこと以外は実施例4と同様にして接合体を作製した。
Comparative Example 3 A joined body was produced in the same manner as in Example 4 except that the double-sided pressure-sensitive adhesive tape obtained in Comparative Example 1 was used. Comparative Example 4 A joined body was produced in the same manner as in Example 4 except that the double-sided pressure-sensitive adhesive tape obtained in Comparative Example 2 was used.

【0031】上記実施例及び比較例について、以下に示
す方法で評価を行った。 (評価方法) 1.伸度 JISL1096「一般織物試験方法」に準拠して測定
した。 2.100%伸長強度 JISL1096「一般織物試験方法」に準拠して測定
した。 3.PP90度剥離粘着力 JISZ0238に準拠し、実施例1〜3及び比較例1
〜2で得られた両面粘着テープを23℃環境下でPP
(ポリプロピレン)板に貼付け、テープ背面を25μm
PETフィルムにて裏打ちした後、2kgローラーにて
速度300mm/分で一往復して圧着する。張り付け2
4時間後、同環境下でストログラフにて剥離速度300
mm/分の条件で粘着力を測定した。
The above Examples and Comparative Examples were evaluated by the following methods. (Evaluation method) 1. Elongation Measured in accordance with JIS L1096 "General textile test method". 2.100% elongation strength Measured in accordance with JISL1096 "General textile test method". 3. PP 90 degree peel adhesive strength According to JISZ0238, Examples 1 to 3 and Comparative Example 1
The double-sided pressure-sensitive adhesive tape obtained in Steps 2 to 2 was PP
(Polypropylene) affixed to the plate, tape back 25μm
After backing with a PET film, the film is pressed and reciprocated once with a 2 kg roller at a speed of 300 mm / min. Paste 2
After 4 hours, under the same environment, peeling speed 300
The adhesive strength was measured under the condition of mm / min.

【0032】4.80℃定荷重剥離力 実施例1〜3及び比較例1〜2で得られた両面粘着テー
プより切出された巾20mm、長さ50mmの試料を、
23℃の環境下で、PP(ポリプロピレン)板に2kg
ローラーにて速度300mm/分で圧着し、テープ背面
を25μmPETフィルムにて裏打ちした後、24時間
放置後80℃環境下に投入し、図2に示すようにテープ
片端に80gの荷重をかけ、3時間後の剥離量を測定す
ることにより剥離力を判断した。 5.接合体評価 実施例4〜6、比較例3〜4にて得られた接合体を80
℃環境下に投入し、240時間放置後、接合体の部材1
と部材2との接合面における浮き・剥がれの状態を目視
確認した。上記による測定評価結果は表1及び表2に示
すとおりであった。
4. 80 ° C. Constant Load Peeling Force A 20 mm wide and 50 mm long sample cut from the double-sided pressure-sensitive adhesive tape obtained in Examples 1 to 3 and Comparative Examples 1 and 2 was used.
2kg in PP (polypropylene) plate under 23 ℃ environment
After pressure-bonding with a roller at a speed of 300 mm / min, backing the tape back with a 25 μm PET film, leaving it for 24 hours, put it in an environment of 80 ° C., apply a load of 80 g to one end of the tape as shown in FIG. The peeling force was determined by measuring the amount of peeling after time. 5. Bonded body evaluation The bonded bodies obtained in Examples 4 to 6 and Comparative Examples 3 to 4 were 80
C. environment, left for 240 hours, then joined member 1
The state of floating and peeling at the joint surface between the member and the member 2 was visually confirmed. The measurement and evaluation results as described above were as shown in Tables 1 and 2.

【0033】[0033]

【表1】 [Table 1]

【0034】[0034]

【表2】 表1及び2から明らかなように、本発明における実施例
においては、高いPP粘着力を有し、定荷重下における
剥離量においても優れた剥離強度を有するとともに、接
合体においても浮きや剥がれが発生しないことが判明し
た。
[Table 2] As is clear from Tables 1 and 2, in the examples of the present invention, while having high PP adhesive strength, having excellent peel strength even in the amount of peeling under a constant load, floating and peeling also occur in the joined body. It was found not to occur.

【0035】[0035]

【発明の効果】本発明の両面粘着テープは、曲面追従性
を有する不織布を用いるので、複雑な形状の付着体に追
従しやすく、被着体からの剥離強度を大幅に向上するこ
とができるとともに、被着体がオレフィン樹脂系部材で
あっても、充分な剥離強度を得ることができる。また、
特定の伸度及び伸長強度を有する不織布、或いは粘着層
が、特定のアクリル系共重合体を主成分とするアクリル
系粘着剤を用いた場合には、上記効果を更に確実に奏し
うる。更に、本発明における接合体は、上記両面粘着テ
ープを用いて接合されてなるので、複雑な凹凸形状を有
する部材や、オレフィン樹脂系部材を用いた場合であっ
ても、接合界面で浮きや剥がれのない接合体を得ること
が可能となる。
As the double-sided pressure-sensitive adhesive tape of the present invention uses a nonwoven fabric having a curved surface followability, it can easily follow an adherend having a complicated shape, and can greatly improve the peel strength from the adherend. Even if the adherend is an olefin resin-based member, sufficient peel strength can be obtained. Also,
When the nonwoven fabric having a specific elongation and the elongation strength or the pressure-sensitive adhesive layer uses an acrylic pressure-sensitive adhesive containing a specific acrylic copolymer as a main component, the above effects can be more reliably exerted. Furthermore, since the joined body in the present invention is joined using the above-mentioned double-sided adhesive tape, even if a member having a complicated uneven shape or an olefin resin-based member is used, it floats or peels off at the joining interface. It becomes possible to obtain a joined body without any.

【図面の簡単な説明】[Brief description of the drawings]

【図1】本発明の接合体の一例を示す模式図である。FIG. 1 is a schematic view showing an example of a joined body of the present invention.

【図2】実施例における80℃定荷重剥離力の測定方法
を示す模式図である。
FIG. 2 is a schematic diagram showing a method for measuring a constant load peeling force at 80 ° C. in an example.

【符号の説明】[Explanation of symbols]

1.部材1 2.部材2 3.両面粘着テープ 1. Member 1 2. Member 2 3. Double-sided adhesive tape

Claims (4)

【特許請求の範囲】[Claims] 【請求項1】 曲面追従性を有する不織布の両面に粘着
層が設けられてなることを特徴とする両面粘着テープ。
1. A double-sided pressure-sensitive adhesive tape comprising a nonwoven fabric having a curved surface followability property and pressure-sensitive adhesive layers provided on both sides.
【請求項2】 不織布が、縦及び横方向の伸度が各10
0%以上であり、100%伸長強度が3N/cm以下で
あることを特徴とする、請求項1記載の両面粘着テー
プ。
2. The nonwoven fabric has an elongation of 10 and 10 in the longitudinal and transverse directions, respectively.
The double-sided pressure-sensitive adhesive tape according to claim 1, wherein the pressure-sensitive adhesive tape has a tensile strength of 0% or more and a 100% elongation strength of 3 N / cm or less.
【請求項3】 粘着層が、炭素数4〜10のアルキル基
を有するアルキル(メタ)アクリレートが30〜95重
量%の割合で含有され共重合されてなるアクリル系共重
合体を主成分とするアクリル系粘着剤からなることを特
徴とする、請求項1又は2記載の両面粘着テープ。
3. A pressure-sensitive adhesive layer comprising, as a main component, an acrylic copolymer obtained by copolymerizing an alkyl (meth) acrylate having an alkyl group having 4 to 10 carbon atoms in a proportion of 30 to 95% by weight. 3. The double-sided pressure-sensitive adhesive tape according to claim 1, comprising an acrylic pressure-sensitive adhesive.
【請求項4】 請求項1〜3の何れか1項記載の両面粘
着テープを用いてポリオレフィン系部材が接合されてな
ることを特徴とする接合体。
4. A joined body obtained by joining polyolefin-based members using the double-sided pressure-sensitive adhesive tape according to claim 1.
JP2001227833A 2001-03-29 2001-07-27 Double-coated adhesive tape and bonded product Pending JP2002356660A (en)