CS263180B1 - Modified asphalt Mm polyolefin - Google Patents

Modified asphalt Mm polyolefin Download PDF

Info

Publication number
CS263180B1
CS263180B1 CS867314A CS731486A CS263180B1 CS 263180 B1 CS263180 B1 CS 263180B1 CS 867314 A CS867314 A CS 867314A CS 731486 A CS731486 A CS 731486A CS 263180 B1 CS263180 B1 CS 263180B1
Authority
CS
Czechoslovakia
Prior art keywords
asphalt
polyethylene
modified
construction
molecular weight
Prior art date
Application number
CS867314A
Other languages
Czech (cs)
Slovak (sk)
Other versions
CS731486A1 (en
Inventor
Alfred Ing Runa
Margita Ing Masarykova
Original Assignee
Runa Alfred
Margita Ing Masarykova
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Runa Alfred, Margita Ing Masarykova filed Critical Runa Alfred
Priority to CS867314A priority Critical patent/CS263180B1/en
Publication of CS731486A1 publication Critical patent/CS731486A1/en
Publication of CS263180B1 publication Critical patent/CS263180B1/en

Abstract

iešenie sa týká nového modifikovaného asfaltu na báze polyolefínu, polyetylénu s ohraničenou molekulovou hmotnosťou. Modifikovaný asfalt sa skládá z 2 % hmot. až 15 % hmot. vysokotlakového polyetylénu s molekulovou hmotnostou v rozmedzí 11 000 až 14 000 a 98 % hmot. až 85 » hmot. ropného asfaltu s penetráciou 25 °C 60 až 150 penetračných jednotiek. Modifikovaný asfalt sa móže výhodné použit ako spojivo pri stavbě mimoriadne zatažených čestných úsekov, či už vo formě asfaltových betónov, liatych asfaltov alebo mastixov a tiež v hydroizolačnom stavitelstve.The solution concerns a new modified asphalt based on polyolefin, polyethylene with a limited molecular weight. Modified asphalt consists of 2% wt. to 15% wt. of high-pressure polyethylene with a molecular weight in the range of 11,000 to 14,000 and 98% wt. to 85% wt. of petroleum asphalt with a penetration at 25 °C of 60 to 150 penetration units. Modified asphalt can be advantageously used as a binder in the construction of extremely loaded road sections, whether in the form of asphalt concrete, cast asphalt or mastics and also in waterproofing construction.

Description

263180 2263180 2

Vynález sa týká nového modifikovaného asfaltu na báze polyolefínu s využitím najma v cestnom stavielstve pri výrobě asfaltových spojiv s vyššou odolnostou voči plastickým deformáciám. Běžné typy komerčně vyrábaných druhov polyetylénov s aplikačným určením pre priemyselplastických hmůt, zvyšujú pri modifikácii asfaltov tvrdosti, /meranú bodom mSknutia podláHilhelmiho /W/ v °C, připadne metodou krúžok-gulička, kde 1 °C W 4 7 až 10 °KGZ při obsahu4,0 % hmot. na asfalt o 5 °C až 7 °C a pri obsahu 8,0 % hmot. na asfalt o 14 °C až 17 °C/Zenke-Hastenbek: Literaturauswertung "Verbesserung des Verformingswiderstandes durchPolymer-modifiziertes Bitumen" 1982 str. 15 a str. 16/. Doterajší světový stav technikypozná použitie polyetylénu na přípravu modifikovaných asfaltov najma v kombinácii s inýmidruhmi plastomérov a elastomérov. Modifikovaný asfalt připravený iba s polyetylénom molekulo-vé j hmotnosti 11 000 až 14 000 nebol doteraz publikovaný. Asfaltová kompozícia, podláMitsubischi Chem. In. JP č. 9 138 263 z 8.8.84 obsahuje nízkomolekulárny polyetylénv kombináci s dalšími zložkami, je určená ako zmes odolná voči působeniu vody. Velká částliteratúry i patentovej je věnovaná technologickým podmienkám přípravy modifikovanýchasfaltov s použitím polyetylénu /NSR 2 363 733, NSR 1 694 052, Francúzsko 232 488,Preil-Scholze: Untersuchungen an thermoplastcompoundieřten Bitumen die Strašse č. 12/76str. 511 a č. 4/77 str. 162/.BACKGROUND OF THE INVENTION The present invention relates to a novel modified polyolefin-based asphalt utilized especially in road construction for the production of asphalt binders with higher resistance to plastic deformation. Conventional types of commercially produced polyethylene with industrial application rates increase the hardness of the bitumen (as measured by the point of intersection with Hilhelmi / W / in ° C) by modifying the asphalt, or by ring-ball method where 1 ° CW 4 7 to 10 ° KGZ at content 4, % Wt. to asphalt by 5 ° C to 7 ° C and at 8.0% by weight; asphalt by 14 ° C to 17 ° C / Zenke-Hastenbek: Literaturauswertung "Verbesserung des Verformingswiderstandes durchPolymer-modifiziertes Bitumen" 1982 pages 15 and 16 /. Prior art will recognize the use of polyethylene for the preparation of modified asphalt, especially in combination with other types of plastomers and elastomers. Modified asphalt prepared only with polyethylene molecular weight of 11,000 to 14,000 has not yet been published. Bituminous composition according to Chem. In. JP No. 9 138 263 of 8.8.84 contains low molecular weight polyethylene in combination with other components, is intended as a water resistant mixture. A large part of the literature and patent is devoted to the technological conditions for the preparation of modified asphalts using polyethylene / NSR 2 363 733, NSR 1 694 052, France 232 488, Preil-Scholze: Untersuchungen an thermoplastic compound Bitumen die Strašse No. 12 / 76p. 511 and No. 4/77 p. 162 /.

Komerčně typy polyetylénov majú molekulovú hmotnost nad 20 000. So zvyšujúcim obsahompolyetylénu ako i so zvyšujúcou sa molekulovou hmotnostou vzrastá úměrně tvrdost modifikované-ho asfaltu, ale súčasne aj viskozita. Pretože obecne vykazujú modifikované asfalty viskozityniekedy o 200 % až 300 8 vyššie hodnoty ako bežne používané komerčně asfalty, vznikájúčasto pri pokládání a hutnění v praxi tažkosti, ktoré v extrémnom případe můžu spůsobit ažnespracovatelnosf modifikovanéj asfaltovej zmesi. V snahe vylepšenia spracovatelnostiasfaltových modifikovaných zmesí sa preto často zvyšuje teplota asfaltového spojiva, čovyžaduje vyššiu spotřebu energie a zvyšuje nebezpečie tepelného znehodnotenia produktu.Commercially, polyethylene types have a molecular weight above 20,000. As both the polyethylene content and the increasing molecular weight increase, the hardness of the modified asphalt increases proportionally, but also viscosity. Since, as a general rule, modified viscosities of viscosity sometimes have from 200% to 300% higher values than commonly used commercially asphalts, they are involved in the laying and compaction in practice of the difficulty which, in the extreme case, can cause unprocessability of the modified asphalt mixture. Therefore, in order to improve processability of bituminous modified compositions, the temperature of the bituminous binder is often increased, requiring higher energy consumption and increasing the risk of thermal deterioration of the product.

Obecne so zvyšováním přídavku polyetylénu klesá pozvolné aj penetrácia /25 °C, tažnosť/-duktilitaZ, bod lámavosti modifikovaného asfaltu. Molekulová hmotnost použitého polyetylénunemá na změnu uvedených ukazatelov taký vplyv ako množstvo přidaného polyméru. Výslednévlastnosti modifikovaného asfaltu su v porovnaní s klasickými asfaltami tej istej penetrač-nej triedy podstatné vyššej kvalitativněj úrovni, čo sa prejavuje najmS zvýšenou odolnostouvoči tepelnému namáhaniu, vylepšenej adhézii ku kamenivu, vysokou odolnostou voči rozpúštaciemuúčinku organických rozpúštadiel, vylepšenými nízkoteplotnými vlastnostem! a najmM získánímelasticity.Generally, as the addition of polyethylene increases, penetration (25 ° C), ductility / ductility (Z), the breaking point of the modified asphalt also decreases slowly. The molecular weight of the polyethylene used to alter the indicated parameters is as much as the amount of polymer added. The resulting properties of the modified asphalt are significantly higher in quality compared to conventional asphalt of the same penetration class, which is manifested in particular by increased resistance to thermal stress, improved adhesion to aggregate, high resistance to solvent dissolution, improved low temperature properties! and at least obtaining the elasticity.

Horeuvedené nedostatky komerčných typov vysokotlakových polyetylénov odstraňuje využitievynálezu.The aforementioned drawbacks of the commercial types of high pressure polyethylenes obviate the use of the invention.

Podstatou vynálezu je modifikovaný asfalt, ktorý sa skládá z 98 % hmot. až 85 8 hmot.asfaltu s penetráciou /25 °C v rozmedzí 60 až 150 pen. jednotiek a z 2 % hmot. až 15 8 hmot.vysokotlakového polyetylénu, vyznačujúci sa tým, že molekulová hmotnost vysokotlakovéhopolyetylénu sa pohybuje v rozmedzí 11 000 až 14 000. Vysoký účinok zvyšovania tvrdosti/vyjádřený bodom máknutia °C/ po přídavku 4,0 8 hmot. na asfalt je 13 °C a po přídavku8,0 8 hmot. je 23 °C. V důsledku zvýšeného účinku je možno pre dosiahnutie určitej konštantnejtvrdosti modifikovaného asfaltu použit nižší obsah vysokotlakého polyetylénu. Ďalšia jehovýhoda spočívá v nižšej viskozite výsledného modifikovaného produktu a to nielen z důvoduznlženého obsahu polymérnej přísady, ale i v důsledku viskozity samotného produktu v porovna-ní s bežne vyrábanými typmi polyetylénov. Konečne prídavok vysokotlakového polyetylénuo molekulovej hmotnosti 11 000 až 14 000 sa prejaví i v skrátení doby rozpúštania přísadyv asfalte. Tento vyšší účinok pri modifikácii asfaltov možno vysvětlit optimálnou chemickouštruktúrou polyetylénu, hlavně dlžkou bočných retazcov ako i stupftom rozvetvenia.SUMMARY OF THE INVENTION The subject of the invention is a modified asphalt consisting of 98 wt. to 85% by weight of asphalt with penetration / 25 ° C in the range of 60 to 150 pen. % and 2 wt. up to 15% by weight of high pressure polyethylene, characterized in that the molecular weight of the high pressure polyethylene is in the range 11,000 to 14,000. the asphalt is 13 ° C and after the addition of 8.0 8 wt. is 23 ° C. Due to the increased effect, a lower high-pressure polyethylene content can be used to achieve a certain constant hardness of the modified asphalt. Another disadvantage is the lower viscosity of the resulting modified product, not only because of the reduced polymer additive content, but also due to the viscosity of the product itself compared to commonly produced polyethylene types. Finally, the addition of high-pressure polyethylene having a molecular weight of 11,000 to 14,000 will also result in a shortening of the time of dissolution of the additive in the asphalt. This higher effect on the modification of the asphalts can be explained by the optimal polyethylene chemical structure, mainly the side chain length as well as the degree of branching.

Vynález je dalej podrobnejšie objasněný v následujúcich príkladoch. 3 263180 Příklad 1The invention is further illustrated in the following examples. 3 263180 Example 1

Do východzieho asfaltu gradácie A-P 65 /bod mSknutia KG 49 °C a penetrácie/ 25 °C 63 pen. jednotiek sa postupné přidávalo pri teplote 160 °C až 170 °C za stálého miešania 4,0 % hmot., 6,0 % hmot. a 8,0 % hmot. rSznych typov vysokotlakových polyetylénov, ktoré sa odlišovali molekulovou hmotnosťou. Vlastnosti vyrobených modifikovaných asfaltov sú uvedené v tabulke č. Iv stipcoch 1 až 6. V snahe zvýraznenia rozdielneho účinku je v štipci I uvedený účinok nízkomolekulárneho polyetylénu, v štipci 2 a 3 účinok nekomerčného s optimál-nou chemickou štruktúrou a v stipcoch 4, 5 a 6 bežne vyrábané druhy polyetylénov. Porovnánímtvrdosti vyrobených modifikovaných asfaltov vidíme, že polyetylén s molekulovou hmotnosťou II 000 až 14 000 zvyšuje tvrdosť modifikovaného asfaltu podstatné viac ako ostatné druhy.Podobné výsledky s nízkomolekulárnym polyetylénom v štipci 1 poukazujú na skutočnosť, žetento druh je vzhladom na tepelnú odolnost nevhodný na modifikáciu asfaltov.Into the initial bitumen gradation A-P 65 / point of drop KG 49 ° C and penetration / 25 ° C 63 pen. 4.0% w / w, 6.0% w / w was continuously added at 160-170 ° C with stirring. % and 8.0 wt. Different types of high-pressure polyethylene, which differ in molecular weight. The properties of the modified asphalts produced are shown in Table IV of the columns 1 to 6. In order to emphasize the different effect, the effect of low molecular weight polyethylene in the column I and the effect of the non-commercial with the optimal chemical structure in columns 2 and 3, and 6 commonly produced polyethylene types. By comparing the hardness of the modified bitumen produced, it can be seen that polyethylene with a molecular weight of II 000 to 14 000 increases the hardness of the modified bitumen to a greater degree than other species. Similar results with low molecular weight polyethylene in column 1 indicate that this species is unsuitable for modification of asphalts due to thermal resistance.

Tabulka č. 1Table 1

Vplyv molekulovej hmotnosti vysokotlakového polyetylénu na vlastnosti modifikovanéhoasfaltu připraveného z asfaltu A-P 65 Štipec 1 23 molek. hmotnost PE_7 420_11 570_13 687 množstvo % hmot. 4 6 10 4 6 8 4 6 8 Bod mSknutia W °C 45 46 53,5 52 57 62,5 52,5 57 61 penetrácia /40 °C 342 287 186 157 102 84 126 95 81 /25 °C 81 69 60 44 38 35 40 35 30 / 2 °C 5 7 11 6 8 8 ” 8 6 5 duktilita /40 °C cm +100 +100 31,5 89 34 30 58 30 27 /25 °C cm +100 +100 26 46,5 9 7,5 33,5 15 6,5 / 2 °C cm 6 5 4 5 2 2,5 5 2,5 2 bod lámavosti °C -10 -14 -8 -10 -12 -14 -12 -10 -12 Tepelná stálost (163 °C, 8 h) hmotnostný úbytok % hmot. 0 0 0 0 0 0 0 0 0 bod mSknutia w °c 49 51 55 53 59 62,5 54 57 63 penetrácia /25 °C 52 49 42 40 34 32 36 34 27 duktilita /25 °C cm 100 89 19 70 7 7 25,5 10 5 bod lámavosti °C -10 -12 -6 -8 -9 -8 -12 -12 -10 zníženie penetrácie % 35,8 29 30 9,1 10,5 8,6 10 3 10 zvýšenie b. mSknutia °C 4 5 1,5 1 2 0 1,5 0 2 Štipec 4 5 6 molek. hmotnost PE 14 153 26 437 40 670 množstvo % hmot. 4 6 8 4 6 8 4 6 8 Bod mSknutia W °C 47 49 52 48 49 53 50,5 54 56 penetrácia /40 °C 165 98 86 140 96 81 166 106 83 /25 °C 42 35 32 44 36 32 43 39 34 / 2 °C 6 6 6 7 6 6 5 4 2 duktilita /40 °C cm +100 47 23 +100 40 34 45,5 38 30,5 /25 °C cm 58 ' 9,5 8,5 76 22,5 10,5 29,5 18 4,5 / 2 °C cm 4,5 3 2 5 3 2 3,5 3 1,5 bod lámavosti °C -10 -8 -6 -8 -8 -7 -10 -10 -8 Tepelná stálost(163 °C, 8 h) hmotnostný úbytok % hmot. 0 0 0 0 0 0 0 0 0 bod mSknutia W °C 49 51,5 53 50 50 55 52 56 57 penetrácia /25 °C 38 31 27 40 33 30 38 34 32 263180Effect of molecular weight of high-pressure polyethylene on the properties of modified bitumen prepared from asphalt A-P 65 Pin 1 23 moles. weight PE_7 420_11 570_13 687 amount by weight 4 6 10 4 6 8 4 6 8 Drop point W ° C 45 46 53.5 52 57 62.5 52.5 57 61 penetration / 40 ° C 342 287 186 157 102 84 126 95 81/25 ° C 81 69 60 44 38 35 40 35 30/2 ° C 5 7 11 6 8 8 ”8 6 5 ductility / 40 ° C cm +100 +100 31.5 89 34 30 58 30 27/25 ° C cm +100 +100 26 46 , 5 9 7.5 33.5 15 6.5 / 2 ° C cm 6 5 4 5 2 2.5 5 2.5 2 breaking point ° C -10 -14 -8 -10 -12 -14 -12 - 10 -12 Heat stability (163 ° C, 8 h) weight loss% w / w 0 0 0 0 0 0 0 0 0 point mWetting w ° c 49 51 55 53 59 62.5 54 57 63 penetration / 25 ° C 52 49 42 40 34 32 36 34 27 ductility / 25 ° C cm 100 89 19 70 7 7 25.5 10 5 breaking point ° C -10 -12 -6 -8 -9 -8 -12 -12 -10 penetration reduction% 35.8 29 30 9.1 10.5 8.6 10 3 10 boost b mSwitching ° C 4 5 1.5 1 2 0 1.5 0 2 Pin 5 5 6 moles. weight PE 14 153 26 437 40 670% wt. 4 6 8 4 6 8 4 6 8 Drop point W ° C 47 49 52 48 49 53 50.5 54 56 penetration / 40 ° C 165 98 86 140 96 81 166 106 83/25 ° C 42 35 32 44 36 32 43 39 34/2 ° C 6 6 6 7 6 6 5 4 2 ductility / 40 ° C cm +100 47 23 +100 40 34 45.5 38 30.5 / 25 ° C cm 58 '9.5 8.5 76 22,5 10,5 29,5 18 4,5 / 2 ° C cm 4,5 3 2 5 3 2 3,5 3 1,5 point breaking point ° C -10 -8 -6 -8 -8 -7 - 10 -10 -8 Thermal stability (163 ° C, 8 h) Weight loss% by weight. 0 0 0 0 0 0 0 0 0 Point of drop W ° C 49 51,5 53 50 50 55 52 56 57 penetration / 25 ° C 38 31 27 40 33 30 38 34 32 263180

Tabulka č. 1 pokračovaní Štipec 4 56 molek. hmotnost PE 14 153 26 437 40 670 množstvo % hmot. 4 6 8 4 6 8 4 6 8 duktilita /25 °C cm 47 5 5 62' 16 7 23 12 3,5 bod lámavosti °C -8 -8 -5 -8 —6 -6 -10 -8 -7 zníženie penetrácie % 9,5 11,4 15,6 9 8,3 6,3 11,6 12,8 6 zvýšenie b. mSknutia °C 2 2,5 1 2 1 2 1,5 2 1Table 1 continued Pinch 4 56 moles. weight PE 14 153 26 437 40 670% wt. 4 6 8 4 6 8 4 6 8 ductility / 25 ° C cm 47 5 5 62 '16 7 23 12 3.5 breaking point ° C -8 -8 -5 -8 —6 -6 -10 -8 -7 decrease penetration% 9,5 11,4 15,6 9 8,3 6,3 11,6 12,8 6 increase b.

Pozitivny vplyv využitia vynálezu na spracovatelnost modifikovaných asfaltov je zřejmýz údajov uvedených v tabulke č. 2. V prehlade sú uvedené viskozitné údaje modifikovanýchasfaltov, vyrobených z asfaltu A-P 65 a 8,0 % hmot. rĎznych typov polyetylénov, ktorésa líšia molekulovou hmotnostou. Tieto viskozitné údaje sa 3alej porovnávajú s viskozitamiklasických druhov asfaltov A-P 25 a Bx 15 pri spracovatelských teplotách využívaných privýrobě liatych asfaltov.The beneficial effects of the use of the invention on the processability of modified asphalts are shown in Table 2. The viscosity data of modified asphalts made from asphalt A-P 65 and 8.0% by weight are shown in the review. different types of polyethylene, which differ in molecular weight. These viscosity data are further compared with the viscosity-classic asphalt grades A-P 25 and Bx 15 at the processing temperatures utilized by cast asphalt production.

Nameraná tvrdosť klasických asfaltov vyjádřená ako bod mSknutia KG °C asfaltu A-P 25bola 65 °C, Bx 15 bola 74 °C.The measured hardness of classical asphalts, expressed as the point of dropping KG ° C of the A-P 25bola asphalt 65 ° C, Bx 15 was 74 ° C.

Tabulka č. 2Table 2

Teplota °C 200 220Temperature ° C 200 220

Zloženie ViskozitaPa. s % A-P 25 % Bx 15 Viskozita Pa.s % A-P 25 % Bx 15 klasický asfalt A-P 25 0,085 8 100 - 0,053 6 100 - klasický asfalt Bx 15 0,16 - 100 0,080 - 100 A-P 65 + 8,0 % hmot. PE Mv 40 670 0,295 343 184 0,174 324 217 A-P 65 + 8,0 % hmot. PE 0,123 143 77 0,085 158 100 Mv 26 434 A-P 65 + 8,0 % hmot. PE 0,101 118 63 0,075 140 94 Mv 13 670 A-P 65 + 8,0 % hmot. PE 0,080 5 94 50 0,05 93 62,5 Mv 13 670Composition ViscosityPa. with% A-P 25% Bx 15 Viscosity Pa.s% A-P 25% Bx 15 classical asphalt A-P 25 0.085 8 100 - 0.053 6 100 - classical asphalt Bx 15 0.16 - 100 0.080 - 100 A-P 65 + 8.0% wt. PE Mv 40 670 0.295 343 184 0.174 324 217 A-P 65 + 8.0 wt. PE 0.123 143 77 0.085 158 100 Mv 26 434 A-P 65 + 8.0 wt. PE 0.101 118 63 0.075 140 94 Mv 13 670 A-P 65 + 8.0 wt. PE 0.080 5 94 50 0.05 93 62.5 Mv 13 670

Porovnáním tvrdostí modifikovaných asfaltov z tab. č. 1 s viskozitnými údajmi tab. č. 2je zřejmé, že využitím polyetylénu podlá vynálezu sa pri výrobě modifikovaných asfaltovrovnakej tvrdosti dosahuje pri zníženom obsahu modifikátora spracovatelnosť obdobná akou klasického asfaltu A-P 25, připadne lepžia ako u tvrdšieho asfaltu Bx 15. Z tabulky č. 3, v ktorej je uvedená časová závislost rozpúštania rĎznych druhov vysoko-tlakých polyetylénov v závislosti na ich molekulovéj hmotnosti v množstve 8,0 % hmot.v asfalte A-P 65 pri t = 170 °C vyplývá, že využitím vynálzu sa homogenízuje navrhovanýpolyetylén v asfalte za velmi krátku dobu.By comparing the hardness of modified asphalts from Tab. 1 with viscosity data tab. 2 shows that the use of polyethylene according to the invention, in the production of modified asphalt-hardness hardness, is similar to that of classical asphalt AP 25 at reduced content of modifier, possibly better than harder bitumen Bx 15. Table 3, which shows the time dependence The dissolution of various types of high-pressure polyethylene depending on their molecular weight of 8.0% by weight in asphalt AP 65 at t = 170 ° C suggests that by using the inventive homogeneity of the proposed polyethylene in asphalt in a very short time.

Tabulka č. 3 Molekulová hmotnost polyetylénu Čas (min.) % 40 670 120 100 14 153 55 46 13 687 30 25 11 570 30 25 7 420 15 12,5Table 3 Molecular weight of polyethylene Time (min.)% 40 670 120 100 14 153 55 46 13 687 30 25 11 570 30 25 7 420 15 12.5

Claims (1)

5 263180 Vylepšenie odolnosti modifikovaných asfaltov voči plastickým deformaciám v závislosti na množstve přidávaného polyetylénu v asfalte gradácie A-P 65 a počte zatažení meranej na přístroji trvalých deformácii pri 40 °C vyplývá z tabulky č. 4. Tabulka č. 4 Počet Spojivo/deformácia mm prejazdov A-P 65 Bx 15 A-P 65+ 6 % PE A-P 65+ 8 « ; 465 1,8 0,8 0,5 0,3 930 2,6 1,2 0,7 0,5 1 860 3,9 1,5 1,2 0,7 3 720 - 2,0 1,5 1,3 5 580 - 3,3 1,8 1,7 Asfalty modifikované vysokotlakovým polyetylénom sa využívajú přednostně pri stavběmimoriadne zatažených čestných úsekov, Či už vo formě asfaltových betónov, asfaltovýchmastixov alebo liatych asfaltov ako napr. pri výstavbě městských riadených křižovatkách,parkoviskách alebo autobusových zástavkách. Ďalej sa tieto asfaltové výrobky využívajúv hydroizolačnom stavitelstve, najmS v kombinácii so syntetickými kaučukmi, připadne privýrobě asfaltových hmót pre Speciálně druhy aplikácii v stavebníctVe. PREDMET VYNÁLEZU Modifikovaný asfalt, ktorý sa skládá z 98 % až 85 % hmot. asfaltu s penertáciou /25 °Cv rozmedzí 60 až 150 pen. jednotiek a z 2 % až 15 % hmot. vysokotlakového polyetylénuvyznačujúoi sa tým, že molekulová hmotnost vysokotlakového polyetylénu sa pohybuje v rozmedzí11 000 až 14 000.5 263180 Improved plastic deformation resistance of modified asphalts depending on the amount of polyethylene added in the AP 65 asphalt gradation and the number of retracts measured on the permanent deformation apparatus at 40 ° C is shown in Table 4. Table No. 4 Binder / deformation mm AP passages 65 Bx 15 AP 65+ 6% PE AP 65+ 8 «; 465 1.8 0.8 0.5 0.3 930 2.6 1.2 0.7 0.5 1,860 3.9 1.5 1.2 0.7 3 720 - 2.0 1.5 1 , 3 5 580 - 3,3 1,8 1,7 High-pressure polyethylene-modified bitumen is used preferentially in the construction of exceptionally retracted sections of honor, whether in the form of asphalt concrete, asphalt or asphalt, such as for the construction of urban controlled junctions, car parks or bus. flag. Furthermore, these asphalt products are used in waterproofing construction, in particular in combination with synthetic rubbers, possibly for the production of asphalt masses for special types of construction applications. OBJECT OF THE INVENTION Modified asphalt consisting of 98% to 85% wt. of asphalt with a penetration / 25 ° C in the range of 60 to 150 pen. % of the units and from 2% to 15% by wt. high pressure polyethylene, characterized in that the molecular weight of the high pressure polyethylene ranges from about 11,000 to about 14,000.
CS867314A 1986-10-09 1986-10-09 Modified asphalt Mm polyolefin CS263180B1 (en)