CN87101195A - 一种探伤用着色渗透液 - Google Patents

一种探伤用着色渗透液 Download PDF

Info

Publication number
CN87101195A
CN87101195A CN87101195.6A CN87101195A CN87101195A CN 87101195 A CN87101195 A CN 87101195A CN 87101195 A CN87101195 A CN 87101195A CN 87101195 A CN87101195 A CN 87101195A
Authority
CN
China
Prior art keywords
dye penetrant
red
azophloxine
orchil
penetrant
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Withdrawn
Application number
CN87101195.6A
Other languages
English (en)
Other versions
CN1010615B (zh
Inventor
陈时宗
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
HUDONG SHIPYARD
Original Assignee
HUDONG SHIPYARD
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by HUDONG SHIPYARD filed Critical HUDONG SHIPYARD
Priority to CN 87101195 priority Critical patent/CN1010615B/zh
Publication of CN87101195A publication Critical patent/CN87101195A/zh
Publication of CN1010615B publication Critical patent/CN1010615B/zh
Expired legal-status Critical Current

Abstract

一种用于无损检测的,不同于传统的探伤着色渗透液。其特征在于:该种着色渗透液不仅可以用有机溶液清洗,也可以用水清洗,而且两种清洗方法的检测灵敏度都能超过传统的探伤着色渗透液的检测灵敏度,可测出最小裂纹开口宽度为0.4μm并能提高测试结论的可靠性。这种新型着色渗透液的发明,方便了实际使用中的操作和技术管理,降低了测试成本。本发明适用于金属、致密性非金属材料及其制件表面缺隙的检测。

Description

一种探伤用着色渗透液,属于用在无损检测中的渗透检测材料。
通常用于表面缺陷无损检测的渗透液,包括着色渗透液和荧光渗透液。都是按渗透液的清洗方法分为:水洗型、后乳化型、溶剂清洗型三类。不仅国内这样分,国外也是这么分的。例如美国标准MIL-I-25135C83年版、日本标准JISZ-2343    83年版、西德标准DIN54150、54152中的有关规定。现在能查到的国外有权威的标准都是这么分的。这样分的原因在于以往没有一种探伤用着色渗透液既能用水清洗,又能用有机溶剂清洗。如日本荣进株式会社的溶剂清洗型渗透液、西德赫林公司水洗型渗透液、国内HD-RS溶剂清洗型渗透液。
必须特别指出的是,原有的着色渗透液在使用过程中存在以下二个问题:
(1)水洗型渗透液、溶剂清洗型渗透液的灵敏度较低,而水洗型渗透液更低。
(2)水洗型和溶剂清洗型渗透液相互之间不可混用清洗液,即不能用有机溶剂去清洗水洗型渗透液,否则会造成“过洗”,降低检测灵敏度至使检测结果失败。相反,用水去清洗溶剂清洗型渗透液,会造成观察衬度下降,又会使灵敏度降低。
本发明的目的是配制一种探伤用着色渗透液。这种着色渗透液既能用水清洗,又能用溶剂清洗。而且两种清洗方法的检测灵敏度均能超过原有的溶剂清洗型渗透液,从而解决上述问题(1)和(2)。
本发明的要点在于在原HD-RS125溶剂清洗型渗透液中加入红色染料和混合助剂,参照专用工艺配制的着色渗透液。
红色染料除原渗透液中的4偶氮红、玫瑰红之外,还加入了3#偶氮红、耐晒红、中性红,其中耐晒红和中性红可以单独使用或配用,通过多种染料拼色,籍以提高检测灵敏度,形成了初步改进的着色渗透液,然后再加入混合助剂。
混合助剂包括表面活性剂、增塑剂、阻燃剂。
表面活性剂常用的有6501椰子油烷基二乙醇酰胺、MOA高级脂肪醇聚氧乙烯醚、JFC、JFCS烷基苯酚聚氧乙烯醚、JU烷基苯酚醚,可任选其中一种配入。
增塑剂有邻苯二甲酸二甲酯、邻苯二甲酸二乙酯、邻苯二甲酸二丙酯,邻苯二甲酸二丁酯,可任选其中一种配入。
阻燃剂有磷酸甲酯、磷酸乙酯、磷酸丙酯、磷酸丁酯,可任选其中一种配入。阻燃剂除阻燃之外,尚有增稠的功能。
本发明与现有技术相比,有显著的积极效果。红色染料相互串激,提高了发色能力;不同颜色互补可以获得较好的色相、色深和鲜明度,因而综合观测效果良好。
另外,在实际的渗透探伤场合中,往往有如下情况:有些场合允许使用水作清洗液,以利操作和降低成本。还有些场合没有方便的水作清洗液,例如野外工地、高空、井下等环境使用时不如采用有机溶剂作清洗液方便。有一些场合根本不允许用水清洗,例如害怕水蚀的精密电气仪器。还有一些场合不允许使用有机溶剂清洗,例如不能接触有机溶剂的氧气贮器管道。由于以前设有一种符合上述各种情况的探伤用着色渗透液既能用水清洗又能用溶剂清洗,因此,探伤人员必须同时备置水洗型和溶剂清洗型的着色渗透液以及它们专门的清洗液。使用实践证明各种溶液是不能混用的,否则会大大降低渗透检验结论的可靠性。而事实上在探伤操作中混用又难免发生。这给操作和技术管理带来很多不便。本发明的积极效果在于只用一种探伤用着色渗透液,很好地解决了上述问题,避免了混用所造成的不良效果。因此,不仅便于使用操作、改善技术管理、降低测试成本,而且对提高着色探伤结论的可靠性有良好的作用。
下面将原有的日本荣进株式会社的溶剂清洗型、西德赫林公司的水洗型、国内HD-RS125溶剂清洗型渗透液和本发明在不混用清洗液和混用清洗液时各种检测灵敏度比较结果列表如下:
不混用清洗 混用清洗
溶剂清洗型渗透液日本荣进株式会社 ≥0.5μm ≥5μm
溶剂清洗型渗透液中国HD-RS125 ≥0.5μm ≥5μm
水洗型渗透液西德赫林公司 ≥2μm ≥10μm
本发明渗透液 ≥0.4μm 不会发生
本发明适用于金属、致密性非金属材料及其制件表面缺隙的检测。
实施例一:
a、原有的HD-RS125溶剂清洗型着色渗透液:
①乙酸    50%
②活性剂TX-10    17%
③邻苯二甲酸二甲酯    18%
④乙二醇醚    15%
⑤玫瑰红    10g/100ml
⑥4#偶氮红    1g/100ml
b、在上述原有的着色渗透液中加入红色染料,形成初步改进的着色渗透液。
①耐晒红    10g/100ml
②3#偶氮红    5g/100ml
c、取初步改进的着色渗透液    75%
再加入混合助剂    25%
Figure 87101195_IMG2
实施例二:
a、原有的HD-RS125溶剂清洗型着色渗透液:
①异丙醇    76%
②活性剂TX-10    6%
③邻苯二甲酸二乙酯    3%
④乙二醇醚    15%
⑤玫瑰红    2g/100ml
⑥4#偶氮红    1g/100ml
b、在上述原有着色渗透液中加入红色染料,形成初步改进的着色渗透液。
①耐晒红    8g/100ml
②3#偶氮红    1g/100ml
c、取初步改进的着色渗透液    80%
再加入混合助剂    20%
Figure 87101195_IMG3
实施例三:
a、原有的HD-RS125溶剂清洗型着色渗透液:
①乙醇    65%
②活性剂TX-10    15%
③邻苯二甲酸二丙酯    5%
④乙二醇醚    15%
⑤玫瑰红    8g/100ml
⑥4#偶氮红    2g/100ml
b、上述原有着色渗透液中加入红色染料,形成初步改进的着色渗透液。
①耐晒红    8g/100ml
②3偶氮红 2g/100ml
c、取初步改进的着色渗透液    78%
再加入混合助剂    22%
Figure 87101195_IMG4
实施例四:
a、原有的HD-RS125溶剂清洗型着色渗透液:
①异丙醇、丁醇    68%
②活性剂TX-10    10%
③邻苯二甲酸二乙酯    8%
④乙二醇醚    14%
⑤玫瑰红    5g/100ml
⑥4#偶氮红    1g/100ml
b、上述原有着色渗透液中加入红色染料,形成初步改进的着色渗透液。
①耐晒红    5g/100ml
②3#偶氮红    1g/100ml
c、取初步改进的着色渗透液    76%
再加入混合助剂    24%
Figure 87101195_IMG5
实施例五:
a、原有的HD-RS125溶剂清洗型着色渗透液:
①乙酸、丁醇    70%
②活性剂TX-10    15%
③邻苯二甲酸二丙酯    1%
④乙二醇醚    14%
⑤玫瑰红    6g/100ml
⑥4#偶氮红    0.1g/100ml
b、上述原有着色渗透液中加入红色染料,形成初步改进的着色渗透液。
①耐晒红    6g/100ml
②3#偶氮红    2.5g/100ml
c、取初步改进的着色渗透液    79%
再加入混合助剂    21%
Figure 87101195_IMG6

Claims (4)

1、一种探伤用着色渗透液其特征是在原有的着色渗透液中加入红色染料和混合助剂配制而成的着色渗透液。
2、按权利要求1所述,红色染料为3#偶氮红、耐晒红、中性红;其混合助剂为表面活性剂、增塑剂、阻燃剂。
3、按权利要求1和2所述,表面活性剂为JFC、JFCS、JU、6501、MOA;增塑剂为邻苯二甲酸二甲酯、邻苯二甲酸二乙酯、邻苯二甲酸二丙酯、邻苯二甲酸二丁酯;阻燃剂为磷酸甲酯、磷酸乙酯、磷酸丙酯、磷酸丁酯。
4、按权利要求1所述,着色渗透液配方的重量百分比如下:
a、①乙醇、异丙醇、丁醇、苯甲醇中任取几种:  80-42%
②活性剂TX  5-20%
③邻苯二甲酸酯  1-18%
④乙二醇醚  14-20%
⑤玫瑰红  1-10g/100ml
⑥4偶氮红 0.1-6g/100ml
b、上述原有配方加入红色染料,形成初步改进的着色渗透液。
①3#偶氮红  0.1-5g/100ml
②耐晒红、中性红两者可单独使用或配用  1-10g/100ml
c、取初步改进的着色渗透液75%-80%,再加入混合助剂25-20%。
Figure 87101195_IMG1
CN 87101195 1987-12-18 1987-12-18 一种探伤用着色渗透液 Expired CN1010615B (zh)