CN1715334A - High efficiency anti-collapse asphalt powder for well drilling liquid - Google Patents

High efficiency anti-collapse asphalt powder for well drilling liquid Download PDF

Info

Publication number
CN1715334A
CN1715334A CN 200510200458 CN200510200458A CN1715334A CN 1715334 A CN1715334 A CN 1715334A CN 200510200458 CN200510200458 CN 200510200458 CN 200510200458 A CN200510200458 A CN 200510200458A CN 1715334 A CN1715334 A CN 1715334A
Authority
CN
China
Prior art keywords
collapse
high efficiency
asphalt
well drilling
drilling liquid
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN 200510200458
Other languages
Chinese (zh)
Other versions
CN1305966C (en
Inventor
倪红霞
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Karamay Aoze Industry And Trade Co ltd
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CNB2005102004582A priority Critical patent/CN1305966C/en
Publication of CN1715334A publication Critical patent/CN1715334A/en
Application granted granted Critical
Publication of CN1305966C publication Critical patent/CN1305966C/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The high efficiency anti-collapse asphalt powder consists of asphalt 62-75 wt%, softening point regulator 0-6 wt%, fluid loss reducing agent 20-35 wt%, and asphalt binding agent 0-5 wt%. The softening point regulator is one or several of calcium chloride, calcium carbonate, calcium oxide and calcium bicarbonate; the asphalt binding agent is water dispersable oil soluble resin and/or sulfonated phenolic resin; and the fluid loss reducing agent is one or several of NF98-7 amine salt dimmer, sulfonated lignite, potassium humate and sulfonated tanning extract. The high efficiency anti-collapse asphalt powder for well drilling fluid has the features of high asphalt content, high softening point, and fineness of 100-400 mesh, and is especially suitable for use in drilling deep well of 3500-8000 m.

Description

High efficiency anti-collapse asphalt powder for well drilling liquid
Technical field
The present invention relates to the pitch class anti-collapse and anti-falling filtration agent of use in the oil field drilling fluids production, is a kind of high efficiency anti-collapse asphalt powder for well drilling liquid and production method thereof and using method.
Background technology
At present, drilling fluid uses pitch class anti-collapse and anti-falling filtration agent product softening temperature all between 40-140 ℃, be applicable to the well of 40-140 ℃ of well temperature, (being that well depth is below 5000m), and, creaming mudstone serious at ultra deep well (more than the 5000m) wellbore stability difficulty, well slough phenomenon influences problems such as property of drilling fluid; Require asphalt content height, softening temperature height, the pitch class anti-collapse and anti-falling filtration agent that adapts to the high temperature deep well stratum is not also appeared in the newspapers at present.
Summary of the invention
The invention provides a kind of high efficiency anti-collapse asphalt powder for well drilling liquid and production method thereof and user, it has high temperature filtration reduction energy, its softening temperature height, and the asphalt content height is adapted to the well of well depth more than 3500 meters especially, and the highest adaptation well depth is 8000 meters
One of technical scheme of the present invention realizes by following measure: a kind of high efficiency anti-collapse asphalt powder for well drilling liquid, it consists of 62% to 75% pitch by weight percentage, 0 to 6% softening temperature conditioning agent, 20% to 35% fluid loss agent, 0 to 5% pitch wedding agent; Wherein, above-mentioned softening temperature conditioning agent is one or more in calcium chloride, lime carbonate, calcium oxide and the Calcium hydrogen carbonate, above-mentioned pitch wedding agent is one or both in water dispersible oil-soluble resin, the sulfonated phenol formaldehyde resin, and above-mentioned fluid loss agent is one or more in NF98-7 double focusing amine salt, sulfonated lignite, potassium humate, the sulfonation tannin extract.
Two of technical scheme of the present invention realizes by following measure: a kind of above-mentioned high efficiency anti-collapse asphalt powder for well drilling liquid production method, it is undertaken by following step: at first be heated to 100 ℃ to 120 ℃ dissolvings in the pitch adding asphalt tank with aequum, to the pitch wedding agent that wherein adds aequum, behind the softening temperature conditioning agent, mix and be cooled to solid at normal temperatures, then be crushed to fineness between 100 order to 400 orders, obtain work in-process, to the fluid loss agent that wherein adds requirement, puddle and evenly obtain needed high efficiency anti-collapse asphalt powder for well drilling liquid again.
Three of technical scheme of the present invention realizes by following measure: a kind of above-mentioned high efficiency anti-collapse asphalt powder for well drilling liquid production method, it is undertaken by following step: at first pitch, pitch wedding agent, the softening temperature conditioning agent with aequum mixes in a quantity as required, through mixed grind and extruding, be crushed to fineness between 100 order to 400 orders by high pressure overhang roll mill, the work in-process that obtain, to the fluid loss agent that wherein adds requirement, puddle and evenly obtain needed high efficiency anti-collapse asphalt powder for well drilling liquid again.
Four of technical scheme of the present invention realizes by following measure: a kind of above-mentioned high efficiency anti-collapse asphalt powder for well drilling liquid production method, it is undertaken by following step: at first pitch, pitch wedding agent, softening temperature conditioning agent and the fluid loss agent with aequum mixes in proportion, through mixed grind and extruding, be crushed to fineness between 100 order to 400 orders by high pressure overhang roll mill, obtain needed high efficiency anti-collapse asphalt powder for well drilling liquid.
Five of technical scheme of the present invention realizes by following measure: a kind of using method of above-mentioned high efficiency anti-collapse asphalt powder for well drilling liquid, it is undertaken by following step: in drilling process, by adding 20 kilograms to 50 kilograms of above-mentioned high efficiency anti-collapse asphalt powder for well drilling liquid amounts in per 1000 kilograms of mud.
High efficiency anti-collapse asphalt powder for well drilling liquid of the present invention has asphalt content height (〉=60%) (oil soluble composition height (〉=60%)), softening temperature height (80-200 ℃), the fineness characteristics of (according to aboveground needs) between the 100-400 order, the present invention is adapted to the well of well depth more than 3500 meters especially, and the highest adaptation well depth is 8000 meters.Production method of the present invention and using method are convenient to operation, and be easy to implement.
The embodiment system
The present invention is not subjected to the restriction of following embodiment, can determine concrete embodiment according to technical scheme of the present invention and practical situation.
Below in conjunction with embodiment the present invention is further described:
Embodiment 1, and this high efficiency anti-collapse asphalt powder for well drilling liquid consists of 62% pitch by weight percentage, 2% softening temperature conditioning agent, 35% fluid loss agent, 1% pitch wedding agent; This high efficiency anti-collapse asphalt powder for well drilling liquid is detected the result who obtains as following table:
Project Index
Outward appearance Black powder
Moisture, % 1.0
Fineness (120 mesh sieve screen over-size), % 1.0
Asphalt content, % 61.0
Relative inhibition (5%KCI relatively) 0.42
Softening temperature, ℃ 140
Embodiment 2, and this high efficiency anti-collapse asphalt powder for well drilling liquid consists of 70% pitch by weight percentage, 6% softening temperature conditioning agent, 24% fluid loss agent, detect the result who obtains as following table to this high efficiency anti-collapse asphalt powder for well drilling liquid:
Project Index
Outward appearance Black powder
Moisture, % 1.0
Fineness (120 mesh sieve screen over-size), % 2.0
Asphalt content, % 70.0
Relative inhibition (5%KCI relatively) 0.32
Softening temperature, ℃ 200
Embodiment 3, and this high efficiency anti-collapse asphalt powder for well drilling liquid consists of 67% pitch by weight percentage, 4% softening temperature conditioning agent, 25% fluid loss agent, 4% pitch wedding agent; This high efficiency anti-collapse asphalt powder for well drilling liquid is detected the result who obtains as following table:
Project Index
Outward appearance Black powder
Moisture, % 1.0
Fineness (180 mesh sieve screen over-size), % 4.0
Asphalt content, % 65.0
Relative inhibition (5%KCI relatively) 0.52
Softening temperature, ℃ 150
Embodiment 4, and this high efficiency anti-collapse asphalt powder for well drilling liquid consists of 65% pitch by weight percentage, 5% softening temperature conditioning agent, 30% fluid loss agent; This high efficiency anti-collapse asphalt powder for well drilling liquid is detected the result who obtains as following table:
Project Index
Outward appearance Black powder
Moisture, % 1.0
Fineness (120 mesh sieve screen over-size), % 1.0
Asphalt content, % 63.0
Relative inhibition (5%KCI relatively) 0.48
Softening temperature, ℃ 160
Embodiment 5, and this high efficiency anti-collapse asphalt powder for well drilling liquid KH-n consists of 73% pitch by weight percentage, 22% fluid loss agent, 5% pitch wedding agent; This high efficiency anti-collapse asphalt powder for well drilling liquid is detected the result who obtains as following table:
Project Index
Outward appearance Black powder
Moisture, % 1.0
Fineness (120 mesh sieve screen over-size), % 3.0
Asphalt content, % 72.0
Relative inhibition (5%KCI relatively) 0.29
Softening temperature, ℃ 98
Embodiment 6, and this high efficiency anti-collapse asphalt powder for well drilling liquid KH-n consists of 75% pitch by weight percentage, 20% fluid loss agent, 1% softening temperature conditioning agent, 4% pitch wedding agent; This high efficiency anti-collapse asphalt powder for well drilling liquid is detected the result who obtains as following table:
Project Index
Outward appearance Black powder
Moisture, % 1.0
Fineness (120 mesh sieve screen over-size), % 2.0
Asphalt content, % 73.0
Relative inhibition (5%KCI relatively) 0.31
Softening temperature, ℃ 121
In the foregoing description 1 to embodiment 6, above-mentioned softening temperature conditioning agent is one or more in calcium chloride, lime carbonate, calcium oxide and the Calcium hydrogen carbonate, above-mentioned pitch wedding agent is one or both in water dispersible oil-soluble resin, the sulfonated phenol formaldehyde resin, and above-mentioned fluid loss agent is one or more in NF98-7 double focusing amine salt, sulfonated lignite, potassium humate, the sulfonation tannin extract.
High efficiency anti-collapse asphalt powder for well drilling liquid in the foregoing description 1 to embodiment 6 can select for use following three kinds of production methods to obtain respectively:
One of its production method is: at first be heated to 100 ℃ or 110 ℃ or 120 ℃ or 100 ℃ to 120 ℃ dissolvings in the pitch adding asphalt tank with aequum, behind the pitch wedding agent that wherein adds aequum, softening temperature conditioning agent, mix and be cooled to solid at normal temperatures, then be crushed to fineness between 100 orders or 200 orders or 300 orders or 400 orders or 100 order to 400 orders, obtain work in-process, to the fluid loss agent that wherein adds requirement, puddle and evenly obtain needed high efficiency anti-collapse asphalt powder for well drilling liquid again.
Two of its production method is: at first pitch, pitch wedding agent, the softening temperature conditioning agent with aequum mixes in a quantity as required, through mixed grind and extruding, be crushed to fineness between 100 orders or 200 orders or 300 orders or 400 orders or 100 order to 400 orders by high pressure overhang roll mill, the work in-process that obtain, to the fluid loss agent that wherein adds requirement, puddle and evenly obtain needed high efficiency anti-collapse asphalt powder for well drilling liquid again.
Three of its production method: at first pitch, pitch wedding agent, softening temperature conditioning agent and the fluid loss agent with aequum mixes in proportion, through mixed grind and extruding, be crushed to fineness between 100 orders or 200 orders or 300 orders or 400 orders or 100 order to 400 orders by high pressure overhang roll mill, obtain needed high efficiency anti-collapse asphalt powder for well drilling liquid.
The using method of the foregoing description 1 to embodiment 6 resulting high efficiency anti-collapse asphalt powder for well drilling liquid of the present invention is: in drilling process, by adding 20 kilograms or 30 kilograms or 40 kilograms or 50 kilograms of above-mentioned high efficiency anti-collapse asphalt powder for well drilling liquid amounts in per 1000 kilograms of mud.
Draw the key technical indexes such as the following table of high efficiency anti-collapse asphalt powder for well drilling liquid of the present invention by the foregoing description:
Project Index
Outward appearance Black powder
Moisture, % ≤10.0
Fineness (120 mesh sieve screen over-size), % ≤10.0
Asphalt content, % ≥60.0
Relative inhibition (5%KCI relatively) ≤1.0
Softening temperature, ℃ 80-200℃
Have asphalt content height (〉=60%) (oil soluble composition height (〉=60%)), softening temperature height (80-200 ℃), fineness (according to aboveground needs) between the 100-400 order by above-mentioned detected result high efficiency anti-collapse asphalt powder for well drilling liquid of the present invention as can be known, it is adapted to the well of well depth more than 3500 meters, the highest adaptation well depth is 8000 meters, and after aboveground application, effect is fine.
High efficiency anti-collapse asphalt powder for well drilling liquid of the present invention is as follows with the control test result of similar other products such as sulfonated gilsonite dry powder and rock asphalt:
The key technical indexes contrast Sulfonated gilsonite dry powder Rock asphalt The present invention
State Dry powder Dry powder Dry powder
Asphalt content, % ≥25 ≥60 ≥60
Water-soluble, % ≥65 ≥20 ≥25
Pitch softening point, ℃ Do not have 80-140 80-200
Fineness (120 mesh sieve surplus), % ≤10 ≤60 ≤10
Price, unit/ton 6400 8900 8900
Anti-collapse speed and effect Softening point value is indeterminate, and asphalt content is low, causes anti sloughing effectiveness general The softening temperature height, the asphalt content height causes anti sloughing effectiveness good The softening temperature height, the asphalt content height causes anti sloughing effectiveness good
The scope of application 40-140 ℃ of well temperature 80-140 ℃ of well temperature 80-200 ℃ of well temperature
Learn that by last table contrast high efficiency anti-collapse asphalt powder for well drilling liquid of the present invention has following characteristics:
1, asphalt content: high efficiency anti-collapse asphalt powder for well drilling liquid of the present invention is all the same high with the asphalt content of rock asphalt powder, and its asphalt content is 〉=60%, but 2.4 times of sulfonated gilsonite dry powder, and the anti-collapse and anti-falling filtration effect is very good.
2, softening temperature: the softening temperature of high efficiency anti-collapse asphalt powder for well drilling liquid of the present invention is 80-200 ℃, and sulfonated gilsonite dry powder does not have softening temperature, the softening temperature of rock asphalt powder is 80-140 ℃, the scope that the softening temperature that high efficiency anti-collapse asphalt powder for well drilling liquid of the present invention is described surpasses them is 140-200 ℃, this has determined the use range of high efficiency anti-collapse asphalt powder for well drilling liquid of the present invention to be: 80-200 ℃ of well temperature, thus fill up the blank (well depth decision well temperature) of 140-200 ℃ of asphalt anti-collapse fluid loss agent.
3, fineness (120 mesh sieve surplus): 120 mesh sieve surpluses of high efficiency anti-collapse asphalt powder for well drilling liquid of the present invention are≤10, can be by the demand of the used 100 mesh sieve cloth of drilling well, and rock asphalt then is difficult to will produce the phenomenon of sticking with paste wire screen by 100 mesh sieve cloth.
The detection method of the pitch class anti-collapse and anti-falling filtration agent of high efficiency anti-collapse asphalt powder for well drilling liquid in the foregoing description and drilling fluid use at present all adopts GB or national sector standard to carry out, and is specific as follows: GB/T 4507-84 pitch softening point testing method (ring and ball method), GB6678-2003 Chemicals sampling general provisions, GB/T260 petroleum products aquametry, SY/T5490-90 drilling fluid test sodium bentonite, SY/T5664-94 shale-control agent for drilling fluid sulfonated gilsonite FT1, SY/T5621-93 drilling fluid test procedure, the SY/T5559 drilling fluid general test method of treatment agent.

Claims (5)

1. high efficiency anti-collapse asphalt powder for well drilling liquid is characterized in that consisting of by weight percentage 62% to 75% pitch, 0 to 6% softening temperature conditioning agent, 20% to 35% fluid loss agent, 0 to 5% pitch wedding agent; Wherein, above-mentioned softening temperature conditioning agent is one or more in calcium chloride, lime carbonate, calcium oxide and the Calcium hydrogen carbonate, above-mentioned pitch wedding agent is one or both in water dispersible oil-soluble resin, the sulfonated phenol formaldehyde resin, and above-mentioned fluid loss agent is one or more in NF98-7 double focusing amine salt, sulfonated lignite, potassium humate, the sulfonation tannin extract.
2. one kind according to the described high efficiency anti-collapse asphalt powder for well drilling liquid production method of claim 1, it is characterized in that being undertaken: at first be heated to 100 ℃ to 120 ℃ dissolvings in the pitch adding asphalt tank with aequum by following step, behind the pitch wedding agent that wherein adds aequum, softening temperature conditioning agent, mix and be cooled to solid at normal temperatures, then be crushed to fineness between 100 order to 400 orders, obtain work in-process, to the fluid loss agent that wherein adds requirement, puddle and evenly obtain needed high efficiency anti-collapse asphalt powder for well drilling liquid again.
3. one kind according to the described high efficiency anti-collapse asphalt powder for well drilling liquid production method of claim 1, it is characterized in that being undertaken by following step: at first pitch, pitch wedding agent, the softening temperature conditioning agent with aequum mixes in a quantity as required, through mixed grind and extruding, be crushed to fineness between 100 order to 400 orders by high pressure overhang roll mill, the work in-process that obtain, to the fluid loss agent that wherein adds requirement, puddle and evenly obtain needed high efficiency anti-collapse asphalt powder for well drilling liquid again.
4. one kind according to the described high efficiency anti-collapse asphalt powder for well drilling liquid production method of claim 1, it is characterized in that being undertaken by following step: at first pitch, pitch wedding agent, softening temperature conditioning agent and the fluid loss agent with aequum mixes in proportion, through mixed grind and extruding, be crushed to fineness between 100 order to 400 orders by high pressure overhang roll mill, obtain needed high efficiency anti-collapse asphalt powder for well drilling liquid.
5. high efficiency anti-collapse asphalt powder for well drilling liquid using method that obtains in described according to claim 1 or 2 or 3 or 4, it is characterized in that being undertaken: in drilling process, by adding 20 kilograms to 50 kilograms of above-mentioned high efficiency anti-collapse asphalt powder for well drilling liquid amounts in per 1000 kilograms of mud by following step.
CNB2005102004582A 2005-08-08 2005-08-08 High efficiency anti-collapse asphalt powder for well drilling liquid Active CN1305966C (en)