CN1287147A - Technological process of producing calcined petroleum coke in coke oven - Google Patents

Technological process of producing calcined petroleum coke in coke oven Download PDF

Info

Publication number
CN1287147A
CN1287147A CN 00112490 CN00112490A CN1287147A CN 1287147 A CN1287147 A CN 1287147A CN 00112490 CN00112490 CN 00112490 CN 00112490 A CN00112490 A CN 00112490A CN 1287147 A CN1287147 A CN 1287147A
Authority
CN
China
Prior art keywords
coke
petroleum coke
coke oven
calcined petroleum
pitch
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN 00112490
Other languages
Chinese (zh)
Other versions
CN1091132C (en
Inventor
苏启善
万红根
柳去迟
罗亦鸣
冯金龙
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
SINOCHEM ZHENJIANG COKING CO Ltd
Original Assignee
ZHENJIANG COKING GAS GROUP CORP
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by ZHENJIANG COKING GAS GROUP CORP filed Critical ZHENJIANG COKING GAS GROUP CORP
Priority to CN00112490A priority Critical patent/CN1091132C/en
Publication of CN1287147A publication Critical patent/CN1287147A/en
Application granted granted Critical
Publication of CN1091132C publication Critical patent/CN1091132C/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

The technological process of producing calcined petroleum coke features the material including delayed petroleum coke and asphalt and four-system production equipment comprising material pre-treatment system, coke oven system for dry distillation and calcination, product post-treatment system and gas-purifying producing system. It can produce calcined petroleum coke with high quality.

Description

The processing method of producing calcined petroleum coke in coke oven
The present invention relates to coal gas and coke making process, belong to a kind of by preparation retard petroleum coke (abbreviation refinery coke) and add pitch, adopt the coking production processing method of producing calcined petroleum coke in coke oven.
Present domestic calcined petroleum coke mainly adopts rotary kiln or pot furnace production technique because the calcined petroleum coke product lumpiness that these two kinds of explained hereafter go out is little, void content is high, intensity is low, and the chemical index of product and trace element are wayward, thereby can not satisfy service requirements effectively, limited further developing of calcined petroleum coke.And traditional coke oven all to produce with coal be metallurgical coke, gasification Jiao or the foundry coke of main raw material, because of considering that coking furnace shaft is produced the adventurous swelling pressure and coke pushing difficulty, in coking production, fugitive constituent, cohesiveness and the coking property of allocating coal charge into all there is strict requirement.Because the cohesiveness and the coking property of retard petroleum coke are all relatively poor, therefore can't on coke oven, produce calcined petroleum coke separately.
Purpose of the present invention just is to overcome the defective that existing calcined petroleum coke is produced, solve coke oven and can not produce the difficult problem of calcined petroleum coke separately with retard petroleum coke, after providing a kind of retard petroleum coke to add pitch, adopt the coking production technology of producing calcined petroleum coke in coke oven by preparation.
Producing calcined petroleum coke in coke oven processing method of the present invention is a raw material with retard petroleum coke and pitch, makes four systems only by raw materials pretreatment, coke oven destructive distillation calcining, product aftertreatment and coal gas and forms:
1, raw material processing system, retard petroleum coke and pitch be respectively through precrushing, is that 70-99%, pitch weight ratio are that the ratio of 1-30% is mixed with belted electronic balance and joined with the retard petroleum coke weight ratio, mixes pulverizing then, and granularity is less than 3mm part 〉=60%;
2, coke oven distillation system through pretreated raw material, is sent into coke oven and is carried out the high temperature carbonization calcining, the control calcining temperature is 950-1350 ℃, and coking time is 12-26 hour, and sophisticated coke is through the cooling quenching, the quenching time is 10-250 second, makes coke temperature≤100 ℃;
3, product after-treatment system, the calcined petroleum coke after coming out of the stove carries out whole grain to granularity, handles through broken, screening, reaches the granularity requirements of 0-150mm, divides packing or ship in bulk;
4, coal gas is made system only, and the coal gas that the high temperature carbonization calcining produces enters the blasting condensation system by coke oven, after gas-liquid separator, condenser, first cold tower, gas blower, electric fishing tower, final cooling tower cooling process, the coal gas after making is only sent.
Processing method the key technical indexes of the present invention and controlled variable are as follows:
One, starting material index
1, retard petroleum coke
Fugitive constituent (%) 7-20
Ash (%) 0.1-1.5
Sulfur (%) 0.35-3.0
Moisture content (%) 1-15
2, pitch
Softening temperature (℃, ring and ball method) 35-180
Ash (%) 0.1-1.5
Fugitive constituent (%) 35-75
Moisture content (%) 1-15
Two, technological process main control parameters
1, raw materials pretreatment system
Broken ingredients by weight proportioning
Retard petroleum coke (%) 70-99
Pitch (%) 1-30
Pulverize back (≤3mm) fineness (%) 〉=60
Go into furnace charge moisture content (%) 1-15
2, coke oven distillation system
Calcining temperature (℃) 950-1350
Coking time (h) 12-26
Quenching time (s) 10-250
Product moisture content (%) 0.1-15
3, product after-treatment system
According to customer requirements, carry out whole grain, handle through broken, screening;
Granularity qualification rate (%)>80
4, coal gas is made system only
Temperature behind the first cold tower (℃)≤40
Blower inlet suction (Pa)≤3000
Clean system back coal gas contains naphthalene amount (mg/NM 3)≤100
Clean system back coal gas tar content (mg/NM 3)≤20
Three, final product quality index
Figure 0011249000071
Annotate: moisture content, granularity can be adjusted according to customer requirements.
When carrying out producing calcined petroleum coke in coke oven, retard petroleum coke and asphalt stock are delivered to the jaw crusher coarse breaking to granularity≤80mm by conveyor, deliver to batch bin respectively through conveyor, then through vibro-feeder or rotary disc feeder control load, measure through electronic belt scale, realize retard petroleum coke and bituminous batching, join the back material and deliver to reaction type pulverizer mixing pulverizing through conveyor, make the compound granularity be crushed to≤3mm partly accounts for more than 60%, deliver to the coke oven furnace top bin through conveyor again, raw material is sent into coke oven carry out destructive distillation by adding coal car, coke oven destructive distillation calcining temperature is 950-1350 ℃, coking time is 12-26 hour.Coke oven also can adopt tamping type coke oven etc. for top dress coke oven.Calcined petroleum coke after the coke oven calcining maturation is pushed into coke guide through pushing machine with coke and enters quenching car again, delivers to the quenching of coke quenching tower water; Also can adopt dry quenching(of coke).The finished product calcined petroleum coke is delivered to the product after-treatment system, carries out whole grain according to customer requirements, through the crusher coarse crushing, sieve then, and granularity qualification rate 〉=80%, product is in bulk or pack shipping to the user.The coal gas that produces during coke oven destructive distillation calcined petroleum coke enters the blasting condensation system, after gas-liquid separator, condenser, first cold tower, gas blower, electric fishing tower, final cooling tower etc. are handled, the coal gas after making is only sent.Processing method of the present invention has the characteristics of following several respects: (1) can use the refinery coke of different size to mix by batch bin to join, refinery coke sulfur, ash, fugitive constituent, trace element into the stokehold are effectively controlled, satisfy the requirement of user quality product; (2) join pitch by mixing, regulated the fugitive constituent of going into furnace charge, improved the coking behavior of raw material, thereby realized the possibility of producing calcined petroleum coke in coke oven; (3) overcome rotary kiln, pot furnace and produced the calcined petroleum coke granularity and determine by raw material, and void content height, the low shortcoming of vibration bulk density; Indexs such as the fineness of processing method of the present invention by regulating furnace charge, fugitive constituent, coke oven temperature just can be produced the calcined petroleum coke of different grain size, void content, intensity and vibration bulk density.
Advantage of the present invention just has been to solve the difficult problem with producing calcined petroleum coke in coke oven, by selecting the retard petroleum coke that is consistent with calcined petroleum coke chemistry, physicals requirement and add pitch and regulate, the indexs such as sulfur, ash, trace element of coke product have been controlled; Improved the coke coking behavior by adding pitch simultaneously; Again by regulating factors such as coke oven temperature and coking time, improved greatly coke granularity and true specific gravity, reduced void content and than resistance, increased intensity and vibration bulk density.And producing calcined petroleum coke is to be based upon on the conventional coking equipment basis of tradition, so coke making process and equipment requirements are simple.Because the calcined petroleum coke quality product obviously improves, thereby its range of application is constantly enlarged, and becomes the important high quality raw material of carbon element industry, aluminium metallurgy industry, chemical industry system gas industry, smelting industry, therefore has marketing prospect widely.
Below in conjunction with accompanying drawing processing method of the present invention is done further: Fig. 1 is a process flow diagram of the present invention.
With reference to accompanying drawing 1, technological process of the present invention comprises first belt feeder 1, first jaw crushing Machine 2, second belt feeder 3, second jaw crusher 4, the 3rd belt feeder 5, pitch feed bin 6, Retard petroleum coke feed bin 7, the 4th belt feeder 8, impact breaker 9, the 5th belt feeder 10, Furnace roof storehouse 11, charging vehicle 12, coke oven 13, quenching tower 14, coke quenching cart 15, gas collection equipment 16, Gas-liquid separator 17, condenser 18, first cold tower 19, air blast 20, electric fishing tower 21, whole Cold tower 22 equipment such as grade. Such as figure, alphabetical A represents that raw material retard petroleum coke, B represent the raw material drop Blue or green, C represents that finished product coke, D represent the rear output coal gas of clean system. First belt in the process equipment Machine 1, first jaw crusher 2, second belt feeder 3, second jaw crusher 4, the 3rd skin Band machine 5, pitch feed bin 6, retard petroleum coke feed bin 7, the 4th belt feeder 8, reaction type fragmentation Machine 9 and the 5th belt feeder 10 consist of the pretreatment of raw material system; Furnace roof storehouse 11, charging vehicle 12, Coke oven 13, quenching tower 14 and coke quenching cart 15 consist of the coke oven distillation system; Product post processing system System is made up of the disintegrating apparatus of routine and screening plant etc.; Gas collection equipment 16, gas-liquid separator 17, condenser 18, first cold tower 19, air blast 20, electric fishing tower 21 and final cooling tower 22 consist of The coal gas cleaning manufacture system. Condenser 18 adopts no filler void tower structure, and gas makes whole through buffering Individual system eliminates the vibration that causes because of turbulent flow and improves purification efficiency.
Below be embodiments of the invention, practical application of the present invention is not limited to and embodiment.
Embodiment 1, adopts producing calcined petroleum coke in coke oven to be used for the coke product of chemical industry
(1) proportioning
Retard petroleum coke account for 82% pitch account for 18% wherein retard petroleum coke require sulfur content≤0.5%, ash≤0.5% according to coke product, therefore select sulfur content≤0.5%, ash≤0.3% of Mixed Delay refinery coke, mix broken fineness≤3mm and account for more than 60%.
(2) coke oven destructive distillation controlled variable
1280 ℃ of coking times of calcining temperature 20 hours
Produce 3 tons/hole of coke output with top dress coke oven.
Coal gas system system only is provided with no filler condenser, and other are identical with conventional coke making process about process control condition.
The main technique specification of equipment is as follows:
1, the first jaw crusher model PE-400 is used for the retard petroleum coke precrushing;
2, the second jaw crusher model PE-400 is used for the pitch precrushing;
3, impact breaker model PFJ-0707 is used for the compound fragmentation;
4, coke oven model 66 types calcining destructive distillation is carried out in this equipment.
Actual coke quality:
1. granularity (mm) 0-150;
2. helium true specific gravity (g/cc) 2.03;
3. void content (%) 35.2;
4. moisture content (%) 4.5;
5. ash (%) 0.3;
6. sulfur (%) 0.48;
7. fugitive constituent (%) 0.55;
8. intensity M40 (%) 75, M10 (%) 9;
9. vibrate bulk density (%) 85;
10. than resistance (* 10 -6Ω m) 545.
Embodiment 2, adopt producing calcined petroleum coke in coke oven to be used for the coke product of aluminium anode
(1) proportioning
Retard petroleum coke account for 90% pitch account for 10% wherein retard petroleum coke require sulfur content≤2.0%, ash≤0.5% according to coke product, therefore select sulfur content≤2.0%, ash≤0.4% of Mixed Delay refinery coke, mix broken fineness≤3mm and account for more than 65%.
(2) coke oven destructive distillation controlled variable
1300 ℃ of coking times of calcining temperature 22 hours
Produce 3 tons/hole of coke output with top dress coke oven.
Coal gas system system only is provided with no filler condenser, and other are identical with conventional coke making process about process control condition.
The main technique specification of equipment is as follows:
1, the first jaw crusher model PE-400 is used for the retard petroleum coke precrushing;
2, the second jaw crusher model PE-400 is used for the pitch precrushing;
3, impact breaker model PFJ-0707 is used for the compound fragmentation;
4, coke oven model 66 types calcining destructive distillation is carried out in this equipment.
Actual coke quality:
1. granularity (mm) 0-130;
2. helium true specific gravity (g/cc) 2.05;
3. moisture content (%) 3.8;
4. ash (%) 0.48;
5. sulfur (%) 1.50;
6. fugitive constituent (%) 0.55;
7. vibrate bulk density (%) 84;
8. than resistance (* 10 -6Ω m) 515.
Embodiment 3, adopt producing calcined petroleum coke in coke oven to be used for the coke product of electrode
(1) proportioning
Retard petroleum coke account for 95% pitch account for 5% wherein retard petroleum coke require sulfur content≤0.8%, ash≤0.5% according to coke product, therefore select sulfur content≤0.8%, ash≤0.4% of Mixed Delay refinery coke, mix broken fineness≤3mm and account for more than 70%.
(2) coke oven destructive distillation controlled variable
1320 ℃ of coking times of calcining temperature 24 hours
Produce 3 tons/hole of coke output with top dress coke oven.
Coal gas system system only is provided with no filler condenser, and other are identical with conventional coke making process about process control condition.
The main technique specification of equipment is as follows:
1, the first jaw crusher model PE-400 is used for the retard petroleum coke precrushing;
2, the second jaw crusher model PE-400 is used for the pitch precrushing;
3, impact breaker model PFJ-0707 is used for the compound fragmentation;
4, coke oven model 66 types calcining destructive distillation is carried out in this equipment.
Actual coke quality:
1. granularity (mm) 0-130;
2. helium true specific gravity (g/cc) 2.08;
3. moisture content (%) 3.5;
4. ash (%) 0.48;
5. sulfur (%) 0.78;
6. fugitive constituent (%) 0.5;
7. vibrate bulk density (%) 87;
8. than resistance (* 10-6 Ω m) 490.
Comparative Examples, the coke product of employing calcined by rotary kiln explained hereafter
Because calcined by rotary kiln explained hereafter coke is uncontrollable to indexs such as true specific gravity, ash, sulfur, void content, fugitive constituent and intensity, so the coke product quality of this Comparative Examples rotary kiln production only is one concrete batch a index.
1. granularity (mm)≤20;
2. true specific gravity (g/cc)≤2.03;
3. void content (%) 〉=45;
4. moisture content (%)≤0.5;
5. ash (%)≤0.5;
6. sulfur (%)≤1.5;
7. fugitive constituent (%)≤0.6;
8. intensity M40 (%)-, M10 (%)-;
9. vibrate bulk density (%) 81;
10. than resistance (* 10-6 Ω m) 600.
Calcined by rotary kiln technology is compared with the coke product that processing method of the present invention is produced
Contrast project coke oven calcining process calcined by rotary kiln technology
(1) granularity (mm) 0-150≤20
(2) true specific gravity (g/cc) 〉=2.00≤2.03
(3) void content (%)≤36 〉=45
(4) intensity
M40(%) ≥75 -
M10 (%)≤9-by contrast as can be known, the every quality index of the coke product of explained hereafter of the present invention is controlled, and granularity and intensity improves greatly, void content reduces greatly, and quality product is obviously improved.

Claims (5)

1, a kind of producing calcined petroleum coke in coke oven processing method is characterized in that with retard petroleum coke and pitch be raw material, makes four systems only by raw materials pretreatment, coke oven destructive distillation calcining, product aftertreatment and coal gas and forms:
(1) raw material processing system, retard petroleum coke and pitch be respectively through precrushing, is that 70-99%, pitch weight ratio are that the ratio of 1-30% is mixed with belted electronic balance and joined with the retard petroleum coke weight ratio, mixes pulverizing then, and granularity is less than 3mm part 〉=60%;
(2) coke oven distillation system through pretreated raw material, is sent into coke oven and is carried out the high temperature carbonization calcining, the control calcining temperature is 950-1350 ℃, and coking time is 12-26 hour, and sophisticated coke is through the cooling quenching, the quenching time is 10-250 second, makes coke temperature≤100 ℃;
(3) product after-treatment system, the calcined petroleum coke after coming out of the stove carries out whole grain to granularity, handles through broken, screening, reaches the granularity requirements of 0-150mm, divides packing or ship in bulk;
(4) coal gas is made system only, and the coal gas that the high temperature carbonization calcining produces enters the blasting condensation system by coke oven, after gas-liquid separator, condenser, first cold tower, gas blower, electric fishing tower, final cooling tower cooling process, the coal gas after making is only sent.
2, producing calcined petroleum coke in coke oven processing method according to claim 1 is characterized in that calcined petroleum coke proportioning retard petroleum coke accounts for 82%, and pitch accounts for 18%.
3, producing calcined petroleum coke in coke oven processing method according to claim 1 is characterized in that calcined petroleum coke proportioning retard petroleum coke accounts for 90%, and pitch accounts for 10%.
4, producing calcined petroleum coke in coke oven processing method according to claim 1 is characterized in that calcined petroleum coke proportioning retard petroleum coke accounts for 95%, and pitch accounts for 5%.
5, producing calcined petroleum coke in coke oven processing method according to claim 1 is characterized in that coal gas makes the system condensing device only and adopt no filler void tower structure.
CN00112490A 2000-08-29 2000-08-29 Technological process of producing calcined petroleum coke in coke oven Expired - Fee Related CN1091132C (en)