CN1181985C - 用透光立体图案玻璃镀镜的生产方法 - Google Patents

用透光立体图案玻璃镀镜的生产方法 Download PDF

Info

Publication number
CN1181985C
CN1181985C CNB031197078A CN03119707A CN1181985C CN 1181985 C CN1181985 C CN 1181985C CN B031197078 A CNB031197078 A CN B031197078A CN 03119707 A CN03119707 A CN 03119707A CN 1181985 C CN1181985 C CN 1181985C
Authority
CN
China
Prior art keywords
glass
plate glass
patterns
flat plate
plating
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CNB031197078A
Other languages
English (en)
Other versions
CN1440880A (zh
Inventor
熊国祥
李金钟
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Henghao Glass Technology Co., Ltd., Shanghai
Original Assignee
HENGHAO GLASS TECHNOLOGY Co Ltd SHANGHAI
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by HENGHAO GLASS TECHNOLOGY Co Ltd SHANGHAI filed Critical HENGHAO GLASS TECHNOLOGY Co Ltd SHANGHAI
Priority to CNB031197078A priority Critical patent/CN1181985C/zh
Publication of CN1440880A publication Critical patent/CN1440880A/zh
Application granted granted Critical
Publication of CN1181985C publication Critical patent/CN1181985C/zh
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

本发明涉及一种采用化学酸腐蚀法生产透光立体图案玻璃镀镜的生产方法,先将透明平板玻璃清洗干净,晾干后用设计好图案的丝网在其上印刷图案,印刷油墨采用防腐油墨,将晾干后印有图案的平板玻璃背面用防腐材料覆盖好后进行单面乳化,将乳化后的平板玻璃清洗后,放进腐蚀液中浸泡10-20分钟,然后将处理后的平板玻璃用水冲洗,清除油墨和玻璃背面的覆盖材料,干燥后制成透光立体图案玻璃,将透光立体图案玻璃按镀镜要求进行化学镀银、镀铝或镀铜,最后干燥、喷漆、洗净制成成品,本工艺一改传统的制镜选材,而使用透光立体图案玻璃进行再镀镜,使玻璃面呈现出银光的图案镜面玻璃,具有很好的新颖性和艺术性,用于壁柜门、家俱、推拉门、工程等领域。

Description

用透光立体图案玻璃镀镜的生产方法
技术领域:
本发明属于玻璃深加工技术领域,尤其涉及一种采用化学酸腐蚀的方法生产透光立体图案玻璃再镀镜的生产方法,制作出的玻璃图案呈银光闪烁状,并相互点缀。
背景技术:
目前,用工艺图案玻璃镀镜主要是以压花玻璃镀镜为主,但它的图案和玻璃都是一律的银白色,无立体感和层次感,而如果用现市场上已有的乳化图案玻璃镀镜,也同样是镜面全为蒙砂效果,无镜面反射效果,失去了镀镜的价值。
发明内容:
本发明的目的在于克服上述的美中不足,而提供一种采用丝网图案印刷技术在白玻上用强耐腐蚀油墨作保护再化学蚀刻作出透光凸起的透光立体图案玻璃并继续镀镜,而产生出透光立体图案玻璃镜产品。该生产方法有效的把酸蚀玻璃和镀镜工艺有机的结合起来,形成了独特的工艺效果。
本发明的目的是这样实现的:采用的技术方法及步骤如下:
(1)先将透明的平板玻璃清洗干净,凉干后用事先设计好图案的丝网在玻璃上印刷图案,印刷油墨采用防腐油墨,后晾干。
(2)将晾干后印有图案的平板玻璃背面用防腐材料覆盖好后进行单面乳化。
(3)将按步骤(2)处理的平板玻璃简单清洗后(保留油墨图案)放进盛有腐蚀液的腐蚀箱中浸泡10---20分钟,腐蚀液的成分及重量配比为:水65--72份,硫酸5-10份,氢氟酸21-26份。
(4)将按步骤(3)处理后的平板玻璃用水冲洗,清除油墨和玻璃背面的覆盖材料。
(5)将按步骤(4)处理后的平板玻璃用水冲洗干净而制成透光立体图案玻璃。
(6)将步骤(5)作出的成品进入到镀镜生产线的清洗段,进行抛光,离子水清洗、水洗。
(7)将步骤(6)处理好的玻璃再进行化学镀镜。
(8)镀镜后干燥喷漆再干燥清洗,制成成品。
本发明的积极效果如下:
1、在透明的平板玻璃上直接印刷图案,将带图案的平板玻璃进行第一次乳化后,又进行第二次酸蚀,而又保持了油墨图案不脱落不变形,所加工出的图案为凸起透明状,立体效果很强,图案凸起的高度为0.03-0.08毫米之间的高度;
2、凸起的图案是透明的,而图案以外的玻璃平面是乳化的,其产品效果是:整片玻璃图案透明,非图案部分朦胧,透明图案立体感强,层次分明,与无图案部分的乳化效果形成了鲜明的对比。
3、将图案一面进行镀镜后,从玻璃正面呈现出透明的立体图案是镜面银光效果,无图案部分是银白色朦胧效果,两都之间对比分明,层次突出,如银河,似银星,象银花,点缀美好空间,将其用于家俱、壁橱门、工程等领域,具有很强的艺术价值。
具体实施方式:
实施例1:
用透光立体图案玻璃镀镜的生产方法是按照下述方法步骤进行:
(1)将透明的平板玻璃清洗干净,凉干后用事先设计好图案的丝网在玻璃上印刷图案,印刷油墨采用防腐油墨,后晾干。
(2)将晾干后印有图案的平板玻璃背面用防腐材料履盖好后进行单面乳化。
(3)将按步骤(2)处理好的平板玻璃清洗后(保留油墨图案)放进盛有腐蚀液的腐蚀箱中浸泡10分钟,腐蚀液的成分及重量配比配制,水65份,硫酸5份,氢氟酸21份。
(4)将按步骤(3)处理后的平板玻璃用水冲洗,清除油墨和玻璃背面的履盖材料。
(5)将按步骤(4)处理后的平板玻璃用水冲洗干净后而成透光立体图案玻璃。
(6)将步骤(5)制成的玻璃转入镀镜流水线的第一步清洗段,进行抛光,离子水、清水冲洗干净。
(7)接步骤(6)转入化学镀镜段进行镀银、干燥。
(8)接步骤(7)转入喷漆、干燥段。
(9)接步骤(8)转入镜面清洗干燥段,最后制成成品。
实施例2:
透光立体图案玻璃的生产方法是按照下述方法步骤进行:
(1)将透明的平板玻璃清洗干净,凉干后用事先设计好图案的丝网在玻璃上印刷图案,印刷油墨采用防腐油墨,后晾干。
(2)晾干后印有图案的平板玻璃背面用防腐材料覆盖好后进行单而乳化。
(3)将按步骤2处理的平板玻璃清洗后(保留油墨图案)放进盛有腐蚀液的腐蚀箱中浸泡15分钟,腐蚀液的成分及重量配比配制,水67份,硫酸8份,氢氟酸25份。
(4)将按步骤3处理后的平板玻璃用水冲洗,清除油墨和玻璃背面的防腐材料。
(5)将按步骤4处理后的平板玻璃用水冲洗干净,干燥后制成成品。
(6)将步骤(5)制成的玻璃转入镀镜流水线的第一步清洗段,进行抛光,离子水、清水冲洗干净。
(7)接步骤(6)转入化学镀镜段进行镀铝干燥。
(8)接步骤(7)转入喷漆、干燥段。
(9)接步骤(8)转入镜面清洗干燥段,而成透交光立体图案玻璃。
实施例3:
透光立体图案玻璃的生产方法是按照下述步骤进行:
(1)将透明的平板玻璃清洗干净、凉干后用事先设计好图案的丝网在玻璃上印刷图案,印刷油墨采用防腐油墨,后晾干。
(2)晾干后印有图案的平板玻璃背面用防腐材料覆盖好后进行单面乳化
(3)将步骤(2)处理的平板玻璃清洗后(保留油墨图案)放进盛有腐蚀液的腐蚀箱中浸泡20分钟,腐蚀液的成分及重量配比配制:水72份,硫酸10份,氢氟酸26份。
(4)将按步骤(3)处理后的平板玻璃用水冲洗,清除油墨和玻璃背面的防腐材料。
(5)将按步骤(4)处理后的平板玻璃用水冲洗干净,而成透光立体图案玻璃。
(6)将步骤(5)制成的玻璃转入镀镜流水线的第一步清洗段,进行抛光,离子水、清水冲洗干净。
(7)接步骤(6)转入化学镀镜段进行镀铜、干燥。
(8)接步骤(7)转入喷漆、干燥段。
(9)接步骤(8)转入镜面清洗干燥段,最后制成成品。

Claims (1)

1、一种用透光立体图案玻璃镀镜的生产方法,其特征在于:采用的方法及步骤如下:
第一步:先将透明的平板玻璃清洗干净,凉干后用事先设计好图案的丝网在玻璃上印刷图案,印刷油墨采用防腐油墨,后晾干,
第二步:将晾干后印有图案的平板玻璃背面用防腐材料覆盖好后进行单面乳化,
第三步:将按步骤2处理的平板玻璃清洗后,放进盛有腐蚀液的腐蚀箱中浸泡10---20分钟,腐蚀液的成分及重量配比为:水65--72份,硫酸5-10份,氢氟酸21-26份,
第四步:将按步骤3处理后的平板玻璃用水冲洗,清除油墨,和玻璃背面的覆盖材料,
第五步:将按步骤4处理后的平板玻璃用水冲洗干净,干燥后制成透光立体图案玻璃。
第六步:将透光立体图案玻璃装到镀镜生产线的清洗段,按镀镜要求抛光,清洗,干燥。
第七步:进行化学镀银、镀铝或镀铜。
第八步:干燥喷漆,清洗干净制成成品。
CNB031197078A 2003-03-10 2003-03-10 用透光立体图案玻璃镀镜的生产方法 Expired - Fee Related CN1181985C (zh)