CN1172143A - 一种发热剂 - Google Patents

一种发热剂 Download PDF

Info

Publication number
CN1172143A
CN1172143A CN 97106480 CN97106480A CN1172143A CN 1172143 A CN1172143 A CN 1172143A CN 97106480 CN97106480 CN 97106480 CN 97106480 A CN97106480 A CN 97106480A CN 1172143 A CN1172143 A CN 1172143A
Authority
CN
China
Prior art keywords
water
temperature
heat generating
powder
generating agent
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN 97106480
Other languages
English (en)
Inventor
王新波
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN 97106480 priority Critical patent/CN1172143A/zh
Publication of CN1172143A publication Critical patent/CN1172143A/zh
Pending legal-status Critical Current

Abstract

本发明公开了一种发热剂,主要由铁粉、食盐、水、催化剂等组成,并且以木屑作为水的载体,配方中所有的原料都为粉状物质,携带极其方便,使用也相当简单;所选用的原料来源充沛,低廉而且无毒,用完以后也不会产生公害,所以便于推广应用。

Description

一种发热剂
本发明涉及一种发热剂。
众所周知,发热需要能源,研究出在严寒冬季里能温暖人体的热源,对于野外工作者,参加滑冰、滑雪和登山的人员,对身体不适、关节炎患者都有很大的好处,虽然产生热的能源很多,但要满足体积小、重量轻、携带方便、安全可靠并要使用简单、发热时间长,温度容易控制,价格便宜等条件的能源,选择的余地就非常小了。
本发明的目的是:提供一种发热剂,它利用铁在空气中氧化生锈时产生热量的原理,加入催化剂来实现长时间稳定发热。
本发明的技术方案是:一种发热剂,由下列成分混合组成,其成分及重量配比为:
(1).铁粉   50--100;
(2).食盐   1--20;
(3).水     5--30;
(4).催化剂 1--20。
本发明进一步的技术方案是:一种发热剂,由下列成分混合组成,其成分及重量配比为:
(1).铁粉   50--100;
(2).食盐   1--20;
(3).水     5--30;
(4).催化剂 1--20。
上述方案中所述催化剂为活性炭粉;
本发明最理想的技术方案是:一种发热剂,由下列成分混合组成,其成分及重量配比为:
(1).铁粉   50--100;
(2).食盐   1--20;
(3).水     5--30;
(4).催化剂 1--20。
所述催化剂为活性炭粉;
该发热剂还含有另一种催化剂--铝粉,配比为1--5;
该发热剂用木屑来作为水的载体,配比为10--80。
上述反应化学方程式是:
实际生活中,上述反应的速度是相当缓慢的,为了使反应容易发生,本发明选用了多种催化剂,如活性炭粉和铝粉,其实食盐也是起催化作用的成分,通过改变这些催化剂的成分和数量来加快反应的发生并控制反应发生时的温度,并且能在较长时间内保持所需要的温度。
本发明的优点是:
1.本发明选择了常用的原材料作为发热剂原料,价格便宜,体积小,重量轻,携带方便,也容易得到。
2.本发明将水吸收在木屑之中,用木屑来作为水的载体,使配方中所有的原料都成为粉状物质,携带极其方便,使用也相当简单。
3.本发明所选用的原料来源充沛,价廉而且无毒,用完以后也不会产生公害,所以便于推广应用。
下面结合实施例对本发明作进一步的描述:
实施例:一种发热剂,由下列成分混合组成,其成分及重量配比为:
(1).铁粉   50--100;
(2).食盐   1--20;
(3).水     5--30;
(4).催化剂 1--20。
所述催化剂为活性炭粉;
该发热剂还含有另一种催化剂--铝粉,配比为1--5;
该发热剂用木屑来作为水的载体,配比为10--80。
1.称取铁粉80克,食盐10克,木屑40克,水10毫升,活性炭粉10克,铝粉1克;充分混合后灌入塑料袋中,插入温度计;发热剂一定要和空气接触,放入保温筒中,保温筒口敞开,室温为12℃。起始温度从12℃开始,经过5小时达到28℃,并能保持在28℃,在此温度维持4天以上,试验结果如下表:
时间h    0    1    2    3     4    5    6   30   31   50   51   52
温度℃   12   16   19   23   25.5   28   28   28   28   28   28   28
时间h   72   73   74   …   99    100   …
温度℃   28   28   28   …   28     28   …
2.称取铁粉80克,食盐10克,木屑40克,水15毫升,活性炭粉10克,铝粉1克;方法同1.室温是12℃。起始温度从12℃开始,经过4小时达到51℃,最高温度为56℃,稳定在50--54℃的时间为3天以上。试验结果如下表:
时间h    0    1    2    3    4    5    6     7     8    9   10   11
温度℃   12   27   39   46   51   52   53   53.5    54.5   56   54   55
时间h   24   25   26   …   49   50   51   …   73
温度℃   53   53.5   54   …   54   53.5   53.5   52   52
3.称取铁粉80克,食盐10克,木屑40克,水20毫升,活性炭粉10克,铝粉1克;方法同1.室温是12℃。起始温度从12℃开始,2小时后迅速达到55℃,7小时到达最高温度69℃,一天后在43℃左右,二天后在38℃左右,三天后在21℃左右,很明显,热稳定性比较差,试验结果如下表:
时间h    0    1    2     3    4    5    6    7    8    9   10   11   12   13   14
温度℃   12   30   55   59.5   61   63   65   69   67   66   65   60   57   52   48
时间h   15   16   17   …   24   25   26   48   49   50   72   73   74
温度℃   46   44   42   …   43   44   43   37   38   37   28   29   28
时间h   …   96   97   98   99   …
温度℃   …   21.5   21   21   21   …
4.称取铁粉80克,食盐10克,木屑40克,水15毫升,活性炭粉10克;方法同1.室温是12℃。起始温度从12℃开始,经过一天到达最高温度37℃,并能维持30—37℃三天以上,试验结果如下表:
时间h    0    1    2     3    4    5    6     7     8   20   21    22
温度℃   12   20   25    27.5   30   30   31   31.5   31.5   35   36   35.5
时间h   23   24   …   48   49   50   …   72   73  …
温度℃   36   37   …   35   35   35   …   30.5   30  …
从上述试验结果看,试验1发热剂的最高温度为28℃,稳定在28℃的时间为4天以上;试验2发热剂的最高温度为56℃,稳定在50--54℃的时间为3天以上;试验3发热剂的最高温度达69℃,但稳定性较差;其中试验2的结果是比较理想的,同时50--54℃是人体取暖所需的适宜温度。试验4由于未加铝粉,热稳定温度与试验2相差20℃左右,因此,试验2的配方为发热剂的理想配方。

Claims (4)

1.一种发热剂,其特征在于由下列成分混合组成,其成分及重量配比为:
(1).铁粉  50--100;
(2).食盐  1--20;
(3).水    5--30;
(4).催化剂1--20。
2.根据权利要求1所述的一种发热剂,其特征在于:所述催化剂为活性炭粉。
3.根据权利要求1或2所述的一种发热剂,其特征在于:该发热剂还含有另一种催化剂--铝粉,配比为1--5。
4.根据权利要求1或2所述的一种发热剂,其特征在于:该发热剂用木屑来作为水的载体,配比为10--80。
CN 97106480 1997-06-20 1997-06-20 一种发热剂 Pending CN1172143A (zh)