CN113203776B - Preparation method of carbon fiber ultramicro disc electrode - Google Patents

Preparation method of carbon fiber ultramicro disc electrode Download PDF

Info

Publication number
CN113203776B
CN113203776B CN202110382747.8A CN202110382747A CN113203776B CN 113203776 B CN113203776 B CN 113203776B CN 202110382747 A CN202110382747 A CN 202110382747A CN 113203776 B CN113203776 B CN 113203776B
Authority
CN
China
Prior art keywords
carbon fiber
glass capillary
capillary tube
glass
ultramicro
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN202110382747.8A
Other languages
Chinese (zh)
Other versions
CN113203776A (en
Inventor
钱鸿昌
崔天宇
张达威
常卫卫
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
University of Science and Technology Beijing USTB
Original Assignee
University of Science and Technology Beijing USTB
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by University of Science and Technology Beijing USTB filed Critical University of Science and Technology Beijing USTB
Priority to CN202110382747.8A priority Critical patent/CN113203776B/en
Publication of CN113203776A publication Critical patent/CN113203776A/en
Application granted granted Critical
Publication of CN113203776B publication Critical patent/CN113203776B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

A method for preparing a carbon fiber ultramicro disc electrode. Penetrating carbon fiber filaments through a glass capillary tube by a traction method; sealing one end of a glass capillary tube through which the carbon fiber filaments penetrate, connecting the other end of the glass capillary tube with a vacuum pump, placing the glass capillary tube on a vertical drawing instrument, and straightening out two glass electrodes by controlling parameters; filling epoxy resin into the gap between the inner wall and the carbon fiber filaments at the tip of the glass capillary tube, and polishing the tip of the glass capillary tube to be disc-shaped by using a grinding wheel after the epoxy resin is completely cured; and pouring conductive silver adhesive from the other end of the glass capillary, inserting a copper wire into the glass capillary to be adhered and conducted with the carbon fiber, and placing the glass capillary in an oven to completely dry the conductive silver adhesive. And finally, sealing the orifice of the glass capillary tube at one end of the inserted wire by using hot melt adhesive. The method can improve the preparation efficiency and the yield of the carbon fiber ultramicro disk electrode, realize batch production and reduce the preparation cost. The carbon fiber ultramicro disc electrode prepared by the method has the advantages of smooth end surface, good insulating layer coating effect, short response time and long service life, and is suitable for scanning probes.

Description

Preparation method of carbon fiber ultramicro disc electrode
Technical Field
The invention discloses a preparation method of a carbon fiber ultramicro disk electrode. Belongs to the technical field of electrochemical analysis.
Background
Ultramicroelectrodes refer to a class of electrodes with electrode dimensions of less than 25 microns. Compared with the conventional large electrode with the general size of more than 1mm, the ultramicroelectrode has many better electrochemical characteristics, such as higher mass transfer rate, smaller time constant, shorter response time, higher detection precision and the like. It is therefore an important development in the field of electrochemistry. The ultramicro disk electrode is easier to prepare than other kinds of ultramicro electrodes, so that the ultramicro disk electrode is the one with the widest application at present. The traditional ultramicro disk electrode uses noble metal such as platinum, gold and the like as electrode material, and the preparation method is generally that a metal wire with the diameter of 10 microns or 25 microns is placed at the bottom of a glass capillary tube, the glass capillary tube is heated under negative pressure to be melted and sealed in the glass capillary tube, then the metal wire is connected to a conducting wire from the other side by conductive silver adhesive, and finally the glass capillary tube sealed with the metal wire side is manually grinded and polished to reduce the radius ratio (also called RG value) of the glass tube and the metal wire so as to obtain the ultramicro disk electrode. With the application of ultramicroelectrodes in the fields of biological analysis, electrophysiology and the like, carbon fiber materials with better biocompatibility are paid more and more attention. The carbon fiber ultramicro disc electrode prepared by the method has a plurality of defects, and the method comprises the following steps:
(1) The carbon fiber filaments are very fine and soft, and are often adsorbed with the glass tube by static electricity, so that the carbon fiber filaments are difficult to be placed into the glass tube like metal wires. If the length of the inserted carbon fiber filament is too short, the inserted carbon fiber filament cannot extend out of the closed glass tube region and cannot be conducted with the rear lead, and it is difficult to insert a sufficiently long carbon fiber filament due to electrostatic effect and the breakage tendency of the carbon fiber filament.
(2) If the temperature is too low in the negative pressure heating process, the glass capillary tube cannot be melted and is in sealing fit with the carbon fiber wire, and if the temperature is too high, the carbon fiber wire is burnt, so that the conductivity of the carbon fiber wire is influenced. The operation process is very difficult to control.
(3) Mechanical or manual grinding is time-consuming and labor-consuming, is not easy to master, and has low yield.
Disclosure of Invention
The invention aims to provide a preparation method of a carbon fiber ultramicro disk electrode, which has high efficiency, low cost and simple and convenient operation, aiming at the problems and the defects of the traditional preparation method of the carbon fiber ultramicro disk electrode.
The purpose of the invention can be realized by the following technical scheme:
a preparation method of a carbon fiber ultramicro disc electrode is characterized by comprising the following preparation steps:
a. penetrating carbon fiber filaments through a glass capillary tube by a traction method;
b. sealing one end of a glass capillary tube through which the carbon fiber yarns penetrate, connecting the other end of the glass capillary tube with a vacuum pump, placing the glass capillary tube on a vertical drawing instrument, and straightening to obtain two glass electrodes by controlling parameters;
c. filling epoxy resin into the gap between the inner wall and the carbon fiber filaments at the tip of the glass capillary tube, and polishing the tip of the glass capillary tube to be disc-shaped by using a grinding wheel after the epoxy resin is completely cured;
d. and pouring conductive silver adhesive from the other end of the glass capillary, inserting a copper wire into the glass capillary to be adhered and conducted with the carbon fiber, and placing the glass capillary in an oven to completely dry the conductive silver adhesive. And finally, sealing the orifice of the glass capillary tube at one end of the inserted wire by using hot melt adhesive.
Further, in the step a, the carbon fiber filaments penetrate through the whole glass capillary tube by using a method of drawing the carbon fiber filaments by stainless steel wire adhesion.
Further, in the step b, the electrode tip is prepared by drawing the carbon fiber filaments below the temperature of melting the entrapped carbon fiber filaments by using a vertical drawing instrument.
Further, in the step c, the tip of the glass capillary tube and the inner carbon fiber wire are sealed in an insulation manner by using an epoxy resin potting manner.
Further, in the step d, the drying temperature of the oven is 80 ℃, and the drying time is 48 hours.
Compared with the prior art, the invention has the characteristics and beneficial results that:
1. the method can simply penetrate the whole carbon fiber into the glass capillary, and avoids the problem that the carbon fiber cannot be conducted due to insufficient length of the inserted carbon fiber to the maximum extent.
2. The electrode is drawn by using a vertical drawing instrument, the price of the electrode is far lower than that of a horizontal laser drawing instrument adopted by a large number of current technologies, the yield of the electrode is greatly improved, and meanwhile, the cost is reduced.
3. The carbon fiber wires and the tips of the glass capillary tubes are sealed and insulated by adopting an epoxy resin encapsulation mode, so that the problem of carbon fiber wire scorching caused by high-temperature firing is solved.
Drawings
FIG. 1 is a schematic diagram of the preparation of a carbon fiber ultramicro disk electrode of the present invention,
FIG. 2 is an optical microscope photograph of a 7-micron diameter carbon fiber ultramicro disk electrode tip prepared by the present invention,
FIG. 3 is a cyclic voltammetry curve of a 7-micron-diameter carbon fiber ultramicro disk electrode prepared by the invention in a 1mMol/L ferrocene methanol solution.
Detailed Description
Examples of applications
This example is a 7 micron diameter carbon fiber ultramicro disk electrode prepared using the method of the present invention, which has good end morphology and excellent electrochemical performance. In this example, a glass capillary having an outer diameter of 1.5mm, an inner diameter of 0.86mm and a length of 15cm was used, which was made of borosilicate glass, and a carbon fiber filament having a diameter of 7 μm was drawn using a Narishige PC-10 vertical drawing apparatus, and a drawing weight of 4 pieces of a seed block was used, and the heating output was 67.4% of the total output of the apparatus, and the preparation thereof is schematically shown in FIG. 1. The RG value of the carbon fiber ultramicro disc electrode obtained finally was about 2, and the tip optical microscope photograph thereof is shown in fig. 2. The sample was connected to a CHI900D scanning electrochemical microscope and placed in a 1mMol/L ferrocene methanol solution for cyclic voltammetry curve scanning at a voltage range of 0V to 0.45V, the results of which are shown in FIG. 3.

Claims (1)

1. A preparation method of a carbon fiber ultramicro disc electrode is characterized by comprising the following preparation steps:
a. penetrating carbon fiber filaments through a glass capillary tube by a traction method;
b. sealing one end of a glass capillary tube through which the carbon fiber filaments penetrate, connecting the other end of the glass capillary tube with a vacuum pump, placing the glass capillary tube on a vertical drawing instrument, and straightening out two glass electrodes by controlling parameters;
c. filling epoxy resin into gaps between the inner wall and the carbon fiber filaments with the tips of the glass capillaries, and polishing the tips of the glass capillaries to be disc-shaped by using a grinding wheel after the epoxy resin is completely cured;
d. pouring conductive silver adhesive from the other end of the glass capillary, inserting a copper wire into the conductive silver adhesive, adhering and conducting the copper wire with carbon fibers, placing the conductive silver adhesive in an oven to completely dry the conductive silver adhesive, and finally sealing the orifice of the glass capillary at one end of the inserted wire by using hot melt adhesive;
in the step a, the carbon fiber wire penetrates through the whole glass capillary by using a method of drawing the carbon fiber wire by adhering stainless steel wires;
in the step b, a vertical drawing instrument is used for drawing at the temperature lower than the temperature of melting the carbon fiber yarns wrapped by the glass capillary to prepare an electrode tip;
in the step c, the tip of the glass capillary tube and the internal carbon fiber wire are sealed in an insulating way by using an epoxy resin potting way;
and d, drying the mixture in the oven at the drying temperature of 80 ℃ for 48 hours.
CN202110382747.8A 2021-04-09 2021-04-09 Preparation method of carbon fiber ultramicro disc electrode Active CN113203776B (en)