CN109294237A - The preparation method of high-damping composite environmental-friendly rubber material - Google Patents

The preparation method of high-damping composite environmental-friendly rubber material Download PDF

Info

Publication number
CN109294237A
CN109294237A CN201811035729.7A CN201811035729A CN109294237A CN 109294237 A CN109294237 A CN 109294237A CN 201811035729 A CN201811035729 A CN 201811035729A CN 109294237 A CN109294237 A CN 109294237A
Authority
CN
China
Prior art keywords
parts
rubber
preparation
damping composite
rubber material
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Withdrawn
Application number
CN201811035729.7A
Other languages
Chinese (zh)
Inventor
黄欢
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Sichuan Zhi Chuang Intellectual Property Operation Co Ltd
Original Assignee
Sichuan Zhi Chuang Intellectual Property Operation Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sichuan Zhi Chuang Intellectual Property Operation Co Ltd filed Critical Sichuan Zhi Chuang Intellectual Property Operation Co Ltd
Priority to CN201811035729.7A priority Critical patent/CN109294237A/en
Publication of CN109294237A publication Critical patent/CN109294237A/en
Withdrawn legal-status Critical Current

Abstract

The invention discloses the preparation method of high-damping composite environmental-friendly rubber material, the component including following parts by weight: 35~46 parts of methyl vinyl silicone rubber, 20~30 parts of nanoclay, 12~23 parts of silane coupling agent, 8~11 parts of zinc oxide, 5~7 parts of paraffin, 20~37 parts of carbon black, N- cyclohexyl -3~6 parts of 4-aminodiphenylamine, 11~16 parts of pine tar, 3~4 parts of Sulfur, 8~19 parts of aluminium hydroxide, 22~34 parts of nitrile rubber, 11~16 parts of neoprene, 14~28 parts of magnesia, 9~17 parts of silica.Service efficiency of the present invention is higher, more convenient to use.

Description

The preparation method of high-damping composite environmental-friendly rubber material
Technical field
The present invention relates to environment protection fields, and in particular to the preparation method of high-damping composite environmental-friendly rubber material.
Background technique
Rubber material is a kind of high molecular material that can restore deformation rapidly under large deformation, it is the important of national economy One of basic industry daily, medical provides light industry rubber product to be indispensable in people's daily life;For digging, traffic, The heavy industry such as building, machinery, electronics and new industry provide various rubber system production equipments or rubber components, application are very wide It is general.
In recent years, the rapid development of rubber industry, to rubber product, more stringent requirements are proposed, and rubber material must be towards Functionalization, fining and the direction of diversification are developed.Traditional single rubber material cannot fully meet making for rapid development With requiring.Rubber belong to elastomer lack crystallizing power, intermolecular force is small, and free volume is big, thus its intensity, hardness, The performances such as wear-resisting and tired are not high, so to pass through reinforcement to rubber, improve its performance.
Summary of the invention
Not environmentally and service efficiency is poor the technical problem to be solved by the present invention is to existing rubber material, purpose exists In providing the preparation method of high-damping composite environmental-friendly rubber material, the use of rubber material is solved the problems, such as.
The present invention is achieved through the following technical solutions:
The preparation method of high-damping composite environmental-friendly rubber material, the component including following parts by weight: methyl ethylene silicon 35~46 parts of rubber, 20~30 parts of nanoclay, 12~23 parts of silane coupling agent, 8~11 parts of zinc oxide, 5~7 parts of paraffin, carbon Black 20~37 parts, N- cyclohexyl -3~6 parts of 4-aminodiphenylamine, 11~16 parts of pine tar, 3~4 parts of Sulfur, aluminium hydroxide 8 ~19 parts, 22~34 parts of nitrile rubber, 11~16 parts of neoprene, 14~28 parts of magnesia, 9~17 parts of silica.
The preparation method of high-damping composite environmental-friendly rubber material, the component including following parts by weight: methyl ethylene silicon 38~42 parts of rubber, 25~28 parts of nanoclay, 14~21 parts of silane coupling agent, 9~11 parts of zinc oxide, 6~7 parts of paraffin, carbon Black 22~35 parts, N- cyclohexyl -4~6 parts of 4-aminodiphenylamine, 14~16 parts of pine tar, 3~4 parts of Sulfur, aluminium hydroxide 10 ~17 parts, 24~32 parts of nitrile rubber, 13~15 parts of neoprene, 16~23 parts of magnesia, 1~13 part of silica 1.
The preparation method of high-damping composite environmental-friendly rubber material, the component including following parts by weight: methyl ethylene silicon 40 parts of rubber, 27 parts of nanoclay, 19 parts of silane coupling agent, 10 parts of zinc oxide, 6 parts of paraffin, 33 parts of carbon black, N- cyclohexyl-N- 5 parts of diphenyl-para-phenylene diamine, 15 parts of pine tar, 4 parts of Sulfur, 16 parts of aluminium hydroxide, 29 parts of nitrile rubber, 14 parts of neoprene, oxygen Change 18 parts of magnesium, 2 parts of silica 1.
The present invention the following steps are included:
(1) according to parts by weight than weighing each raw material component;
(2) by methyl vinyl silicone rubber, silane coupling agent, nitrile rubber, neoprene, N- cyclohexyl-N- phenyl pair Phenylenediamine, aluminium hydroxide are added in rubber mixing machine and are kneaded at 80~110 DEG C;
(3) it is added nanoclay in the rubber mixing machine in step (2), zinc oxide, paraffin, pine tar, Sulfur is uniformly mixed Afterwards, it is kneaded 40~60 minutes at 50~70 DEG C, obtains mixing virgin rubber;
(4) to step (magnesia, carbon black, silica is added in the mixing virgin rubber in (3) and stirs 20 at 40~60 DEG C ~30 minutes, then natural cooling, obtained the rubber composite material.
Compared with prior art, the present invention having the following advantages and benefits:
1, the preparation method of high-damping composite environmental-friendly rubber material of the present invention, rubber material of the invention is more environmentally-friendly, more Convenient for being used for a long time;
2, the preparation method of high-damping composite environmental-friendly rubber material of the present invention, service efficiency of the present invention is higher, using more It is convenient.
Specific embodiment
To make the objectives, technical solutions, and advantages of the present invention clearer, below with reference to embodiment, the present invention is made Further to be described in detail, exemplary embodiment of the invention and its explanation for explaining only the invention, are not intended as to this The restriction of invention.
Embodiment 1
The preparation method of high-damping composite environmental-friendly rubber material of the present invention, the component including following parts by weight: methyl second 35~46 parts of alkenyl silicon rubber, 20~30 parts of nanoclay, 12~23 parts of silane coupling agent, 8~11 parts of zinc oxide, paraffin 5~7 Part, 20~37 parts of carbon black, N- cyclohexyl -3~6 parts of 4-aminodiphenylamine, 11~16 parts of pine tar, 3~4 parts of Sulfur, hydrogen-oxygen Change 8~19 parts of aluminium, 22~34 parts of nitrile rubber, 11~16 parts of neoprene, 14~28 parts of magnesia, 9~17 parts of silica.
The preparation method of the high-damping composite environmental-friendly rubber material, the component including following parts by weight: methyl second 38~42 parts of alkenyl silicon rubber, 25~28 parts of nanoclay, 14~21 parts of silane coupling agent, 9~11 parts of zinc oxide, paraffin 6~7 Part, 22~35 parts of carbon black, N- cyclohexyl -4~6 parts of 4-aminodiphenylamine, 14~16 parts of pine tar, 3~4 parts of Sulfur, hydrogen-oxygen Change 10~17 parts of aluminium, 24~32 parts of nitrile rubber, 13~15 parts of neoprene, 16~23 parts of magnesia, silica 1 1~13 Part.
The preparation method of the high-damping composite environmental-friendly rubber material, the component including following parts by weight: methyl second 40 parts of alkenyl silicon rubber, 27 parts of nanoclay, 19 parts of silane coupling agent, 10 parts of zinc oxide, 6 parts of paraffin, 33 parts of carbon black, N- hexamethylene 5 parts of base -4-aminodiphenylamine, 15 parts of pine tar, 4 parts of Sulfur, 16 parts of aluminium hydroxide, 29 parts of nitrile rubber, neoprene 14 Part, 18 parts of magnesia, 2 parts of silica 1.
Above-described specific embodiment has carried out further the purpose of the present invention, technical scheme and beneficial effects It is described in detail, it should be understood that being not intended to limit the present invention the foregoing is merely a specific embodiment of the invention Protection scope, all within the spirits and principles of the present invention, any modification, equivalent substitution, improvement and etc. done should all include Within protection scope of the present invention.

Claims (3)

1. the preparation method of high-damping composite environmental-friendly rubber material, which comprises the following steps:
(1) according to parts by weight than weighing each raw material component;
(2) by methyl vinyl silicone rubber, silane coupling agent, nitrile rubber, neoprene, N- cyclohexyl-N- phenyl to benzene two Amine, aluminium hydroxide are added in rubber mixing machine and are kneaded under;
(3) nanoclay is added in the rubber mixing machine in step (2), zinc oxide, paraffin, pine tar, Sulfur is uniformly mixed, obtains To mixing virgin rubber;
(4) to step (magnesia, carbon black, silica is added in the mixing virgin rubber in (3) and stirs 20~30 at 40~60 DEG C Minute, then natural cooling, obtains the rubber composite material.
2. the preparation method of high-damping composite environmental-friendly rubber material according to claim 1, which is characterized in that the step (2) rubber mixing machine is kneaded at 80~110 DEG C in.
3. the preparation method of high-damping composite environmental-friendly rubber material according to claim 1, which is characterized in that the step (3) it is kneaded 40~60 minutes at 50~70 DEG C in.
CN201811035729.7A 2018-09-06 2018-09-06 The preparation method of high-damping composite environmental-friendly rubber material Withdrawn CN109294237A (en)