CN108912545A - Anti-aging cable packaging material and preparation method thereof - Google Patents
Anti-aging cable packaging material and preparation method thereof Download PDFInfo
- Publication number
- CN108912545A CN108912545A CN201810705525.3A CN201810705525A CN108912545A CN 108912545 A CN108912545 A CN 108912545A CN 201810705525 A CN201810705525 A CN 201810705525A CN 108912545 A CN108912545 A CN 108912545A
- Authority
- CN
- China
- Prior art keywords
- preparation
- packaging material
- cable packaging
- aging
- aging cable
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention discloses a kind of anti-aging cable packaging materials and preparation method thereof, which includes:1) aluminium oxide, neopelex, tea polyphenols and water are subjected to ultrasonic vibration, filter to take filtration cakes torrefaction then composition is made;2) polyvinyl chloride, butadiene-styrene rubber, paraffin, palm oil, isooctyl methacrylate, talcum powder, methylcellulose, composition are mixed so that anti-aging cable packaging material is made.The cable packaging material has excellent anti-aging performance, while the preparation method has the advantages that process is simple and raw material is easy to get.
Description
Technical field
The present invention relates to cables, and in particular, to a kind of anti-aging cable packaging material and preparation method thereof.
Background technique
Cable is mainly made of following four part.Conducting wire center:It is made of high electrical conductivity materials (copper or aluminium).According to laying
Requirement of the use condition to cable softness, the every line heart may be twisted by solid conductor or multiple conducting wires;Insulating layer:
Insulating materials as cable should have high insulation resistance, high breakdown field strength, low dielectric loss and low Jie
Electric constant.Sealing sheath:Protect protection insulated wire heart from the damage of machinery, moisture, moisture, chemical substance, light etc..For moisture-sensitive
Insulation, generally use lead or aluminium extrusion sealing sheath;Protect coating:To protect sealing sheath from mechanical damage.
Existing cable needs to coat packaging film in the external of cable during factory, and existing packaging film is generally PE
Film, has the advantages that a series of, but also suffers from certain drawbacks, will appear aging after coating for a long time such as packaging film, into
And it is caused to be difficult to play the role of protecting cable.
Summary of the invention
The object of the present invention is to provide a kind of anti-aging cable packaging material and preparation method thereof, cable packaging material tools
There is excellent anti-aging performance, while the preparation method has the advantages that process is simple and raw material is easy to get.
To achieve the goals above, the present invention provides a kind of preparation methods of anti-aging cable packaging material, including:
1) aluminium oxide, neopelex, tea polyphenols and water are subjected to ultrasonic vibration, then filter to take filtration cakes torrefaction
Composition is made;
2) by polyvinyl chloride, butadiene-styrene rubber, paraffin, palm oil, isooctyl methacrylate, talcum powder, methylcellulose,
Composition is mixed so that anti-aging cable packaging material is made.
The present invention provides a kind of anti-aging cable packaging material, which passes through upper preparation side
Method is prepared.
In the above-mentioned technical solutions, the present invention is adsorbed in tea polyphenols on aluminium oxide by way of ultrasonic vibration first
Composition is formed, then carries out being mixed to get cable packaging material by composition and other raw materials, cable packaging material tool
There is excellent anti-aging property.
Other features and advantages of the present invention will the following detailed description will be given in the detailed implementation section.
Specific embodiment
Detailed description of the preferred embodiments below.It should be understood that described herein specific
Embodiment is merely to illustrate and explain the present invention, and is not intended to restrict the invention.
The present invention provides a kind of preparation methods of anti-aging cable packaging material, including:
1) aluminium oxide, neopelex, tea polyphenols and water are subjected to ultrasonic vibration, then filter to take filtration cakes torrefaction
Composition is made;
2) by polyvinyl chloride, butadiene-styrene rubber, paraffin, palm oil, isooctyl methacrylate, talcum powder, methylcellulose,
Composition is mixed so that anti-aging cable packaging material is made.
In step 1) of the invention, the dosage of each material can select in a wide range, but in order to further mention
The anti-aging property of high cable packaging material, it is preferable that in step 1), aluminium oxide, neopelex, tea polyphenols and
The weight ratio of water is 50:10-15:6-9:100-150.
In step 1) of the invention, the condition of ultrasonic vibration can select in a wide range, but in order to further
Improve the anti-aging property of cable packaging material, it is preferable that in step 1), ultrasonic vibration meets the following conditions:Supersonic frequency
For 25-30KHz, the concussion time is 40-60min.
In step 1) of the invention, dry condition can select in a wide range, but in order to further increase
The anti-aging property of cable packaging material, it is preferable that in step 1), drying meets the following conditions:Drying temperature is 100-120
DEG C, drying time 2-4h.
In step 2) of the invention, the dosage of each material can select in a wide range, but in order to further mention
The anti-aging property of high cable packaging material, it is preferable that in step 2), polyvinyl chloride, butadiene-styrene rubber, paraffin, palm oil, first
Base Isooctyl acrylate monomer, talcum powder, methylcellulose, composition weight ratio be 60:30-40:16-27:25-30:10-18:
11-15:3-6:18-26.
In step 2) of the invention, mixed condition can select in a wide range, but in order to further increase
The anti-aging property of cable packaging material, it is preferable that in step 2), mixing meets the following conditions:Mixing temperature is 15-35
DEG C, incorporation time 20-40min.
The present invention provides a kind of anti-aging cable packaging material, which passes through upper preparation side
Method is prepared.
The present invention will be described in detail by way of examples below.
Embodiment 1
1) by aluminium oxide, neopelex, tea polyphenols and water according to 50:13:7:130 weight ratio carries out ultrasound
Concussion (supersonic frequency 28KHz, concussion time are 50min), then filtering to take filtration cakes torrefaction, (drying temperature is 110 DEG C, dry
Time is 3h) composition is made;
2) by polyvinyl chloride, butadiene-styrene rubber, paraffin, palm oil, isooctyl methacrylate, talcum powder, methylcellulose,
Composition is according to 60:35:19:28:14:13:5:24 weight ratio is mixed, and (mixing temperature is 25 DEG C, and incorporation time is
30min) anti-aging cable packaging materials A 1 is made.
Embodiment 2
1) by aluminium oxide, neopelex, tea polyphenols and water according to 50:10:6:100 weight ratio carries out ultrasound
Concussion (supersonic frequency 25KHz, concussion time are 40min), then filtering to take filtration cakes torrefaction, (drying temperature is 100 DEG C, dry
Time is 4h) composition is made;
2) by polyvinyl chloride, butadiene-styrene rubber, paraffin, palm oil, isooctyl methacrylate, talcum powder, methylcellulose,
Composition is according to 60:30:16:25:10:11:3:18 weight ratio is mixed, and (mixing temperature is 15 DEG C, and incorporation time is
40min) anti-aging cable packaging materials A 2 is made.
Embodiment 3
1) by aluminium oxide, neopelex, tea polyphenols and water according to 50:15:9:150 weight ratio carries out ultrasound
Concussion (supersonic frequency 30KHz, concussion time are 40min), then filtering to take filtration cakes torrefaction, (drying temperature is 120 DEG C, dry
Time is 2h) composition is made;
2) by polyvinyl chloride, butadiene-styrene rubber, paraffin, palm oil, isooctyl methacrylate, talcum powder, methylcellulose,
Composition is according to 60:40:27:30:18:15:6:26 weight ratio is mixed, and (mixing temperature is 35 DEG C, and incorporation time is
20min) anti-aging cable packaging materials A 3 is made.
Application examples 1
Above-mentioned cable packaging material is kneaded 40min, film forming so that cable packaging film is made, is not added with combination in control group
Object;Then according to GB/T 13022-1991 detection cable packaging film tensile strength 1, above-mentioned packaging film is then placed in 500W's
72h is irradiated under ultraviolet light, then detects the tensile strength 2 of packaging film, finally calculates the change rate of the tensile strength of packaging film, is become
Rate=(tensile strength 1- tensile strength 2)/tensile strength 1 × 100%;Concrete outcome is shown in Table 1.
Table 1
Cable packaging material | A1 | A2 | A3 | Control group |
Change rate/% | 1.8 | 2.2 | 1.6 | 10.3 |
The preferred embodiment of the present invention has been described above in detail, still, during present invention is not limited to the embodiments described above
Detail within the scope of the technical concept of the present invention can be with various simple variants of the technical solution of the present invention are made, this
A little simple variants all belong to the scope of protection of the present invention.
It is further to note that specific technical features described in the above specific embodiments, in not lance
In the case where shield, can be combined in any appropriate way, in order to avoid unnecessary repetition, the present invention to it is various can
No further explanation will be given for the combination of energy.
In addition, various embodiments of the present invention can be combined randomly, as long as it is without prejudice to originally
The thought of invention, it should also be regarded as the disclosure of the present invention.
Claims (7)
1. a kind of preparation method of anti-aging cable packaging material, which is characterized in that including:
1) aluminium oxide, neopelex, tea polyphenols and water are subjected to ultrasonic vibration, filter to take filtration cakes torrefaction then to make
Obtain composition;
2) by polyvinyl chloride, butadiene-styrene rubber, paraffin, palm oil, isooctyl methacrylate, talcum powder, methylcellulose, combination
Object is mixed so that the anti-aging cable packaging material is made.
2. preparation method according to claim 1, wherein in step 1), the aluminium oxide, dodecyl benzene sulfonic acid
The weight ratio of sodium, tea polyphenols and water is 50:10-15:6-9:100-150.
3. preparation method according to claim 1, wherein in step 1), the ultrasonic vibration meets the following conditions:It is super
Acoustic frequency is 25-30KHz, and the concussion time is 40-60min.
4. preparation method according to claim 1, wherein in step 1), the drying meets the following conditions:Dry temperature
Degree is 100-120 DEG C, drying time 2-4h.
5. preparation method according to claim 1, wherein in step 2), polyvinyl chloride, butadiene-styrene rubber, paraffin, palm
Oil, isooctyl methacrylate, talcum powder, methylcellulose, composition weight ratio be 60:30-40:16-27:25-30:
10-18:11-15:3-6:18-26.
6. preparation method according to claim 1, wherein in step 2), the mixing meets the following conditions:Mixing temperature
Degree is 15-35 DEG C, incorporation time 20-40min.
7. a kind of anti-aging cable packaging material, which is characterized in that the anti-aging cable packaging material passes through claim 1-6
Any one of described in preparation method be prepared.