CN108822535A - A kind of the production formula and technique of marble grain - Google Patents

A kind of the production formula and technique of marble grain Download PDF

Info

Publication number
CN108822535A
CN108822535A CN201810550893.5A CN201810550893A CN108822535A CN 108822535 A CN108822535 A CN 108822535A CN 201810550893 A CN201810550893 A CN 201810550893A CN 108822535 A CN108822535 A CN 108822535A
Authority
CN
China
Prior art keywords
nylon
masterbatch
marble grain
injection molding
toner
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201810550893.5A
Other languages
Chinese (zh)
Inventor
刘伟
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Dongguan Mi Chen Industrial Technology Co Ltd
Original Assignee
Dongguan Mi Chen Industrial Technology Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Dongguan Mi Chen Industrial Technology Co Ltd filed Critical Dongguan Mi Chen Industrial Technology Co Ltd
Priority to CN201810550893.5A priority Critical patent/CN108822535A/en
Publication of CN108822535A publication Critical patent/CN108822535A/en
Pending legal-status Critical Current

Abstract

The present invention relates to the production formula and technique of a kind of marble grain, the production formula based on percentage, including:Nylon 12 90-98%, toner 0.01-0.08%, Masterbatch 1-5%, wherein Masterbatch includes:Nylon 12 50-70%, titanium dioxide 20-45% and pigment 1-5%.The manufacture craft includes:Step 1, by the nylon 12 of above-mentioned formula ratio, titanium dioxide and pigment mixed grinding at Masterbatch;The nylon 12, toner, Masterbatch of above-mentioned formula ratio are uniformly mixed by step 2;Mixture is put into dehumidifying heat pump and is dried by step 3;Dried material is put into injection molding in injection molding machine by step 4.By observation, the marble grain nature degree of this programme preparation is high.By the technique of disposable directly injection molding, the fluency of the lines of marble grain and natural smart are good, and the unique texture and sense of touch of marble lines element achieve the effect that parian, jade line.And this programme simplifies production process, one-pass molding is simplified manually, is greatly improved work efficiency.

Description

A kind of the production formula and technique of marble grain
Technical field
The present invention relates to the marble grain technical fields of plastic products, more particularly to a kind of production of marble grain Formula and technique.
Background technique
In recent years, marble grain element is brought to fashion trend with its inherent texture and texture again Top throne.It is mostly to pass through secondary operation after injection molding currently, the marble grain effect of PA12 plastic products in the market.Than Such as glasses, clock and watch temporarily can reach parian, jade surface lines effect by being directly molded without a kind of technology in the market The technology of fruit, be mostly secondary operation after the injection molding such as carving again by CA pressing plate technology technique work it out similar to marble, The decorative pattern of the natural lines such as jade, not only visual effect is false for the product that this secondary operation technology is worked it out, and manufacturing procedure More, artificial amount is big, and lines single effect is mechanical, and there is no the natural texture for perfectly embodying marble grain.Therefore, industry The technique that interior urgent need researches and develops a kind of direct injection molding production marble grain.
Summary of the invention
Not only visual effect is false for the marble grain worked it out for secondary operation technology of the existing technology, Er Qiejia Problem more than work process, the present invention provide the production formula and technique of a kind of marble grain.
The concrete scheme of the application is as follows:
A kind of production formula of marble grain, including:Nylon 12 90-98%, toner 0.01-0.08%, Masterbatch 1- 5%, wherein Masterbatch includes:Nylon 12 50-70%, titanium dioxide 20-45% and pigment 1-5%.
In the present embodiment, based on percentage, including:Nylon 12 95-98%, toner 0.02-0.05%, Masterbatch 2- 4%, wherein Masterbatch includes:Nylon 12 55-65%, titanium dioxide 30-40% and pigment 2-4%.
In the present embodiment, based on percentage, including:Nylon 12 96.94%, toner 0.04%, Masterbatch 3%, In, Masterbatch includes:62% nylon 12,35% titanium dioxide and 3% pigment.
A kind of manufacture craft of marble grain, including:
Step 1, by the nylon 12 of the formula ratio of above-mentioned any one, titanium dioxide and pigment mixed grinding at Masterbatch;
Nylon 12, toner, Masterbatch that step 1 corresponds to the formula ratio of scheme are uniformly mixed by step 2;
Mixture is put into dehumidifying heat pump and is dried by step 3;
Dried material is put into injection molding in injection molding machine by step 4.
In the present embodiment, the drying temperature of the dehumidifying heat pump is 100 DEG C.
In the present embodiment, the drying time is 6-8 hours dry.
In the present embodiment, the drying time is 7 hours dry.
In the present embodiment, the injection temperature is 230 DEG C -260 DEG C.
In the present embodiment, the injection temperature is 240 DEG C.
In the present embodiment, the step of dried material is put into injection molding in injection molding machine, includes:In injection moulding process, use Bolt special is stirred.
Compared with prior art, the present invention has the advantages that:
By observation, the marble grain nature degree of this programme preparation is high.By the technique of disposable directly injection molding, greatly The fluency of the lines of fibrous gypsum texture and natural smart are good, the unique texture and sense of touch of marble lines element, reach imitative big The effect of fibrous gypsum, jade line.And this programme simplifies production process, one-pass molding is simplified manually, and work effect is substantially increased Rate.
Specific embodiment
It in order to make the object, technical scheme and advantages of the embodiment of the invention clearer, below will be in the embodiment of the present invention Technical solution be clearly and completely described, it is clear that described embodiments are some of the embodiments of the present invention, rather than Whole embodiments.Based on the embodiments of the present invention, those of ordinary skill in the art are not making creative work premise Under every other embodiment obtained, shall fall within the protection scope of the present invention.
Embodiment 1
A kind of production formula of marble grain, based on percentage, including:Nylon 12 97.99%, toner 0.01%, color Master batch 2%, wherein Masterbatch includes:Nylon 12 60%, titanium dioxide 38% and pigment 2%.
The manufacture craft of the marble grain, including:
Step 1, by the nylon 12 of above-mentioned formula ratio, titanium dioxide and pigment mixed grinding at Masterbatch;
The nylon 12, toner, Masterbatch of above-mentioned formula ratio are uniformly mixed by step 2;
Mixture is put into dehumidifying heat pump and is dried by step 3;The drying temperature of the dehumidifying heat pump is 100 DEG C. The drying time is 6 hours dry.
Dried material is put into injection molding in injection molding machine by step 4.The injection temperature is 230 DEG C.In injection moulding process In, it is stirred using bolt special.
Embodiment 2
A kind of production formula of marble grain, based on percentage, including:Nylon 12 96%, toner 0.05%, Masterbatch 3.95%, wherein Masterbatch includes:Nylon 12 65%, titanium dioxide 32% and pigment 3%.
The manufacture craft of the marble grain, including:
Step 1, by the nylon 12 of above-mentioned formula ratio, titanium dioxide and pigment mixed grinding at Masterbatch;
The nylon 12, toner, Masterbatch of above-mentioned formula ratio are uniformly mixed by step 2;
Mixture is put into dehumidifying heat pump and is dried by step 3;The drying temperature of the dehumidifying heat pump is 100 DEG C. The drying time is 7 hours dry.
Dried material is put into injection molding in injection molding machine by step 4.The injection temperature is 230 DEG C.In injection moulding process In, it is stirred using bolt special.
Embodiment 3
A kind of production formula of marble grain, based on percentage, including:Nylon 12 95.96%, toner 0.06%, color Master batch 4%, wherein Masterbatch includes:Nylon 12 63%, titanium dioxide 35% and pigment 2%.
The manufacture craft of the marble grain, including:
Step 1, by the nylon 12 of above-mentioned formula ratio, titanium dioxide and pigment mixed grinding at Masterbatch;
The nylon 12, toner, Masterbatch of above-mentioned formula ratio are uniformly mixed by step 2;
Mixture is put into dehumidifying heat pump and is dried by step 3;The drying temperature of the dehumidifying heat pump is 100 DEG C. The drying time is 8 hours dry.
Dried material is put into injection molding in injection molding machine by step 4.The injection temperature is 240 DEG C.In injection moulding process In, it is stirred using bolt special.
Embodiment 4
A kind of production formula of marble grain, based on percentage, including:Nylon 12 97.94%, toner 0.06%, color Master batch 2%, wherein Masterbatch includes:Nylon 12 60%, titanium dioxide 36% and pigment 4%.
The manufacture craft of the marble grain, including:
Step 1, by the nylon 12 of above-mentioned formula ratio, titanium dioxide and pigment mixed grinding at Masterbatch;
The nylon 12, toner, Masterbatch of above-mentioned formula ratio are uniformly mixed by step 2;
Mixture is put into dehumidifying heat pump and is dried by step 3;The drying temperature of the dehumidifying heat pump is 100 DEG C. The drying time is 6 hours dry.
Dried material is put into injection molding in injection molding machine by step 4.The injection temperature is 230 DEG C.In injection moulding process In, it is stirred using bolt special.
Embodiment 5
A kind of production formula of marble grain, based on percentage, including:Nylon 12 96.94%, toner 0.04%, color Master batch 3%, wherein Masterbatch includes:62% nylon 12,35% titanium dioxide and 3% pigment.
The manufacture craft of the marble grain, including:
Step 1, by the nylon 12 of above-mentioned formula ratio, titanium dioxide and pigment mixed grinding at Masterbatch;
The nylon 12, toner, Masterbatch of above-mentioned formula ratio are uniformly mixed by step 2;
Mixture is put into dehumidifying heat pump and is dried by step 3;The drying temperature of the dehumidifying heat pump is 100 DEG C. The drying time is 6 hours dry.
Dried material is put into injection molding in injection molding machine by step 4.The injection temperature is 230 DEG C.In injection moulding process In, it is stirred using bolt special.
By observation, the marble grain nature degree of above-described embodiment 1-5 preparation is high.By being disposably directly molded into The technique of type, the fluency of the lines of marble grain and natural smart are good, the unique texture and touching of marble lines element Sense, achievees the effect that parian, jade line.And this programme simplifies production process, one-pass molding is simplified manually, is mentioned significantly High working efficiency.
The embodiments described above only express several embodiments of the present invention, and the description thereof is more specific and detailed, but simultaneously It cannot therefore be construed as limiting the scope of the patent.It should be pointed out that coming for those of ordinary skill in the art It says, without departing from the inventive concept of the premise, various modifications and improvements can be made, these belong to protection of the invention Range.Therefore, the scope of protection of the patent of the invention shall be subject to the appended claims.

Claims (10)

1. a kind of production formula of marble grain, which is characterized in that based on percentage, including:Nylon 12 90-98%, Toner 0.01-0.08%, Masterbatch 1-5%, wherein Masterbatch includes:Nylon 12 50-70%, titanium dioxide 20-45% and face Expect 1-5%.
2. the production formula of marble grain according to claim 1, which is characterized in that based on percentage, including:Poly- ten Two lactams 95-98%, toner 0.02-0.05%, Masterbatch 2-4%, wherein Masterbatch includes:Nylon 12 55-65%, Titanium dioxide 30-40% and pigment 2-4%.
3. the production formula of marble grain according to claim 2, which is characterized in that based on percentage, including:Poly- ten Two lactams 96.94%, toner 0.04%, Masterbatch 3%, wherein Masterbatch includes:62% nylon 12,35% titanium dioxide and 3% pigment.
4. a kind of manufacture craft of marble grain, which is characterized in that including:
Step 1, by the nylon 12, titanium dioxide and pigment mixed grinding of the formula ratio of claim 1-3 any one at Masterbatch;
The nylon 12, toner, Masterbatch of the formula ratio of step 1 corresponding claims are stirred by step 2 It is even;
Mixture is put into dehumidifying heat pump and is dried by step 3;
Dried material is put into injection molding in injection molding machine by step 4.
5. the manufacture craft of marble grain according to claim 4, which is characterized in that the drying of the dehumidifying heat pump Temperature is 100 DEG C.
6. the manufacture craft of marble grain according to claim 4, which is characterized in that the drying time is dry 6- 8 hours.
7. the manufacture craft of marble grain according to claim 6, which is characterized in that the drying time is dry 7 Hour.
8. the manufacture craft of marble grain according to claim 4, which is characterized in that the injection temperature be 230 DEG C- 260℃。
9. the manufacture craft of marble grain according to claim 8, which is characterized in that the injection temperature is 240 DEG C.
10. the manufacture craft of marble grain according to claim 4, which is characterized in that dried material is put into injection molding Include the step of injection molding in machine:
In injection moulding process, it is stirred using bolt special.
CN201810550893.5A 2018-05-31 2018-05-31 A kind of the production formula and technique of marble grain Pending CN108822535A (en)