CN108505140A - A kind of preparation method of the mosquito-proof bacteriostatic fiber of bamboo charcoal - Google Patents
A kind of preparation method of the mosquito-proof bacteriostatic fiber of bamboo charcoal Download PDFInfo
- Publication number
- CN108505140A CN108505140A CN201810344360.1A CN201810344360A CN108505140A CN 108505140 A CN108505140 A CN 108505140A CN 201810344360 A CN201810344360 A CN 201810344360A CN 108505140 A CN108505140 A CN 108505140A
- Authority
- CN
- China
- Prior art keywords
- bamboo charcoal
- fiber
- bamboo
- mosquito
- proof
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention discloses a kind of preparation methods of the mosquito-proof bacteriostatic fiber of bamboo charcoal, first select old bamboo and are sintered into bamboo charcoal, and bamboo charcoal is then ground into bamboo-carbon powder using gas flow crushing process;Bamboo-carbon powder is equably spilt into the polyester fiber of melting again, if use arterial highway draft process, until each bamboo-carbon powder naked fall obtains bamboo charcoal fiber after polyester fibre surface, spinning;Then the ribes after oil expression are selected, is placed on after being dried under high temperature, is extracted after ribes are ground into tea oil slag using gas flow crushing process, obtain anophelifuge;Finally bamboo charcoal fiber is crimped using crimping device, and anophelifuge is dropped to by bamboo charcoal fiber surface by titration mechanism built-in in crimping device, so that anophelifuge is adsorbed in the micropore of bamboo charcoal fiber, it eventually passes through after thermal finalization is stablized and the mosquito-proof bacteriostatic fiber of bamboo charcoal is made, through the above way, the present invention enables to fiber obtained to have antibacterial, mosquito-proof effect, and non-toxic to humans.
Description
Technical field
The present invention relates to fiber arts, more particularly to a kind of preparation method of the mosquito-proof bacteriostatic fiber of bamboo charcoal.
Background technology
Being constantly progressive and develop with science and technology, requirement of the present people for living standard is also constantly promoted, especially
Showed in the requirement of the home textiles articles for use such as clothing, cotton-wadded quilt it is especially prominent, nowadays, in summer, due to the reason of mosquito so that people
It is required for kindling mosquito repellent incense before sleep being prevented, not only be inconvenient, but also the less effective due to hypertelorism, it is mosquito-proof
Fiber type progresses into market.
Then, mosquito-proof fiber type currently on the market is both needed to realize by pyrethroids mosquito-proof, but the pyrethroids is by right
The insecticidal constituent of the 4 kinds of 0.4-2% contained in Dalmatian chrysanthemum(Pyrethrin first, second and cinerin first, second)Shape after being refined
At, and not only chemical property is unstable for the chrysanthemum of this unartificial synthesis, is easy hydrolysis, there is also toxic defects, are used for a long time
After human body can be damaged.
Invention content
The invention mainly solves the technical problem of providing a kind of preparation methods of the mosquito-proof bacteriostatic fiber of bamboo charcoal, enable to
Fiber obtained has antibacterial, mosquito-proof effect, and non-toxic to humans.
In order to solve the above technical problems, one aspect of the present invention is:A kind of mosquito-proof antibacterial fibre of bamboo charcoal is provided
The preparation method of dimension, specifically comprises the following steps:
(1)Old bamboo is selected, and is sintered into bamboo charcoal, the bamboo charcoal is then ground by bamboo charcoal using gas flow crushing process
Powder;
(2)The bamboo-carbon powder is equably spilt into the polyester fiber of melting, if then use arterial highway draft process, until each bamboo
Charcoal powder naked fall obtains bamboo charcoal fiber after polyester fibre surface, spinning;
(3)Ribes after oil expression are selected, are placed on after being dried under high temperature, using gas flow crushing process by the ribes powder
It is extracted after being broken into tea oil slag, obtains anophelifuge;
(4)Bamboo charcoal fiber is crimped using crimping device, and will be prevented by titration mechanism built-in in the crimping device
Mosquito agent drops to bamboo charcoal fiber surface so that anophelifuge is adsorbed in the micropore of bamboo charcoal fiber, eventually passes through 140-160 DEG C of pine
The mosquito-proof bacteriostatic fiber of bamboo charcoal is made after stablizing in relaxation thermal finalization.
In a preferred embodiment of the present invention, the age of the old bamboo needs 5 years or more.
In a preferred embodiment of the present invention, the grain size of the bamboo-carbon powder is 300-500 nanometers.
In a preferred embodiment of the present invention, in the bamboo charcoal fiber, the weight percent of the bamboo-carbon powder contains
Amount is 1-5%.
In a preferred embodiment of the present invention, the grain size of the tea oil slag is 150-250 nanometers.
In a preferred embodiment of the present invention, the fineness of the mosquito-proof bacteriostatic fiber of the bamboo charcoal is 1.5-11D.
The beneficial effects of the invention are as follows:
1)It can compared to the pyrethroids of traditional unartificial synthesis as anophelifuge raw material by using the ribes after oil expression
Have nontoxic feature, is used for a long time harmless;
2)Bamboo-carbon powder is made by using old bamboo, and can have at bamboo charcoal fiber with polyester fiber melt spinning
Superior fungistatic effect;
3)The adsorption effect having using the micropore of bamboo charcoal fiber makes anophelifuge penetrate into each micropore, and uses thermal finalization will
Anophelifuge is adsorbed in the micropore of bamboo charcoal fiber steadily in the long term, clothes and home textile articles for use made of the fiber, not only right
The mixed bacterias such as Candida albicans, staphylococcus aureus, Escherichia coli, hay bacillus have high fungistatic effect, and
It and can also expelling mosquito so that human body can be from bite by mosquitos.
Specific implementation mode
The preferred embodiments of the present invention will be described in detail below so that advantages and features of the invention can be easier to by
It will be appreciated by those skilled in the art that so as to make a clearer definition of the protection scope of the present invention.
Embodiment 1:
A kind of preparation method of the mosquito-proof bacteriostatic fiber of bamboo charcoal, specifically comprises the following steps:
(1)Old bamboo is selected, and is sintered into bamboo charcoal, the bamboo charcoal is then ground by bamboo charcoal using gas flow crushing process
The grain size of powder, the bamboo-carbon powder is 300 nanometers;
(2)The bamboo-carbon powder is equably spilt into the polyester fiber of melting, then uses 3 draft process, until each bamboo charcoal
Powder naked fall obtains bamboo charcoal fiber after polyester fibre surface, spinning, in the bamboo charcoal fiber, the weight of the bamboo-carbon powder
It is 1% to measure degree;
(3)Ribes after oil expression are selected, are placed on after being dried under high temperature, using gas flow crushing process by the ribes powder
It is extracted after being broken into tea oil slag, the grain size of the tea oil slag is 250 nanometers, obtains anophelifuge;
(4)Bamboo charcoal fiber is crimped using crimping device, and will be prevented by titration mechanism built-in in the crimping device
Mosquito agent drops to bamboo charcoal fiber surface so that anophelifuge is adsorbed in the micropore of bamboo charcoal fiber, eventually passes through 140 DEG C of relaxation heat
The mosquito-proof bacteriostatic fiber of bamboo charcoal is made after stablizing in sizing.
Cotton heterotypic fibre for producing 1.5D*38mm is suitable for shirt, T-shirt, and gained sample is into test, to white
The bacteriostasis rates of the mixed bacterias such as coccus, staphylococcus aureus, Escherichia coli, hay bacillus is read up to 96%.
Embodiment 2:
A kind of preparation method of the mosquito-proof bacteriostatic fiber of bamboo charcoal, specifically comprises the following steps:
(1)Old bamboo is selected, and is sintered into bamboo charcoal, the bamboo charcoal is then ground by bamboo charcoal using gas flow crushing process
The grain size of powder, the bamboo-carbon powder is 350 nanometers;
(2)The bamboo-carbon powder is equably spilt into the polyester fiber of melting, then uses 3 draft process, until each bamboo charcoal
Powder naked fall obtains bamboo charcoal fiber after polyester fibre surface, spinning, in the bamboo charcoal fiber, the weight of the bamboo-carbon powder
It is 2% to measure degree;
(3)Ribes after oil expression are selected, are placed on after being dried under high temperature, using gas flow crushing process by the ribes powder
It is extracted after being broken into tea oil slag, the grain size of the tea oil slag is 220 nanometers, obtains anophelifuge;
(4)Bamboo charcoal fiber is crimped using crimping device, and will be prevented by titration mechanism built-in in the crimping device
Mosquito agent drops to bamboo charcoal fiber surface so that anophelifuge is adsorbed in the micropore of bamboo charcoal fiber, eventually passes through 145 DEG C of relaxation heat
The mosquito-proof bacteriostatic fiber of bamboo charcoal is made after stablizing in sizing.
Medium-length heterotypic fibre for producing 2.5D*51mm, is suitable for dacron drill and blended cotton, and gained sample is into survey
Examination, to the bacteriostasis rates of the mixed bacterias such as Candida albicans, staphylococcus aureus, Escherichia coli, hay bacillus up to 97%.
Embodiment 3:
A kind of preparation method of the mosquito-proof bacteriostatic fiber of bamboo charcoal, specifically comprises the following steps:
(1)Old bamboo is selected, and is sintered into bamboo charcoal, the bamboo charcoal is then ground by bamboo charcoal using gas flow crushing process
The grain size of powder, the bamboo-carbon powder is 400 nanometers;
(2)The bamboo-carbon powder is equably spilt into the polyester fiber of melting, then uses 3 draft process, until each bamboo charcoal
Powder naked fall obtains bamboo charcoal fiber after polyester fibre surface, spinning, in the bamboo charcoal fiber, the weight of the bamboo-carbon powder
It is 3% to measure degree;
(3)Ribes after oil expression are selected, are placed on after being dried under high temperature, using gas flow crushing process by the ribes powder
It is extracted after being broken into tea oil slag, the grain size of the tea oil slag is 200 nanometers, obtains anophelifuge;
(4)Bamboo charcoal fiber is crimped using crimping device, and will be prevented by titration mechanism built-in in the crimping device
Mosquito agent drops to bamboo charcoal fiber surface so that anophelifuge is adsorbed in the micropore of bamboo charcoal fiber, eventually passes through 150 DEG C of relaxation heat
The mosquito-proof bacteriostatic fiber of bamboo charcoal is made after stablizing in sizing.
Wool type heterotypic fibre for producing 3D*64mm, is washed and blended wool spinning fabric suitable for hair, and gained sample is into survey
Examination, to the bacteriostasis rates of the mixed bacterias such as Candida albicans, staphylococcus aureus, Escherichia coli, hay bacillus up to 98%.
Embodiment 4:
A kind of preparation method of the mosquito-proof bacteriostatic fiber of bamboo charcoal, specifically comprises the following steps:
(1)Old bamboo is selected, and is sintered into bamboo charcoal, the bamboo charcoal is then ground by bamboo charcoal using gas flow crushing process
The grain size of powder, the bamboo-carbon powder is 450 nanometers;
(2)The bamboo-carbon powder is equably spilt into the polyester fiber of melting, then uses 3 draft process, until each bamboo charcoal
Powder naked fall obtains bamboo charcoal fiber after polyester fibre surface, spinning, in the bamboo charcoal fiber, the weight of the bamboo-carbon powder
It is 4% to measure degree;
(3)Ribes after oil expression are selected, are placed on after being dried under high temperature, using gas flow crushing process by the tea word powder
It is extracted after being broken into tea oil slag, the grain size of the tea oil slag is 180 nanometers, obtains anophelifuge;
(4)Bamboo charcoal fiber is crimped using crimping device, and will be prevented by titration mechanism built-in in the crimping device
Mosquito agent drops to bamboo charcoal fiber surface so that anophelifuge is adsorbed in the micropore of bamboo charcoal fiber, eventually passes through 155 DEG C of relaxation heat
The mosquito-proof bacteriostatic fiber of bamboo charcoal is made after stablizing in sizing.
Heterotypic fibre for producing 3D-9D*102mm is suitable for Sunday Angora Yarns product, and gained sample is into test, to white
The bacteriostasis rates of the mixed bacterias such as coccus, staphylococcus aureus, Escherichia coli, hay bacillus is read up to 97%.
Embodiment 5:
A kind of preparation method of the mosquito-proof bacteriostatic fiber of bamboo charcoal, specifically comprises the following steps:
(1)Old bamboo is selected, and is sintered into bamboo charcoal, the bamboo charcoal is then ground by bamboo charcoal using gas flow crushing process
The grain size of powder, the bamboo-carbon powder is 500 nanometers;
(2)The bamboo-carbon powder is equably spilt into the polyester fiber of melting, then uses 3 draft process, until each bamboo charcoal
Powder naked fall obtains bamboo charcoal fiber after polyester fibre surface, spinning, in the bamboo charcoal fiber, the weight of the bamboo-carbon powder
It is 5% to measure degree;
(3)Ribes after oil expression are selected, are placed on after being dried under high temperature, using gas flow crushing process by the ribes powder
It is extracted after being broken into tea oil slag, the grain size of the tea oil slag is 150 nanometers, obtains anophelifuge;
(4)Bamboo charcoal fiber is crimped using crimping device, and will be prevented by titration mechanism built-in in the crimping device
Mosquito agent drops to bamboo charcoal fiber surface so that anophelifuge is adsorbed in the micropore of bamboo charcoal fiber, eventually passes through 160 DEG C of relaxation heat
The mosquito-proof bacteriostatic fiber of bamboo charcoal is made after stablizing in sizing.
Heterotypic fibre for producing 9D-11D*65mm is suitable for home textile product, pillow and quilt etc., gained sample
Into test, to the bacteriostasis rates of the mixed bacterias such as Candida albicans, staphylococcus aureus, Escherichia coli, hay bacillus up to 96%.
It should be noted that the age of the old bamboo needs 5 years or more, it can be further ensured that bamboo-carbon powder obtained
Fungistatic effect.
It is different from the prior art, a kind of preparation method of the mosquito-proof bacteriostatic fiber of bamboo charcoal of the present invention, on the one hand, by using warp
Ribes after oil expression can have nontoxic feature as anophelifuge raw material compared to the pyrethroids of traditional unartificial synthesis,
It is used for a long time harmless;On the other hand, be made bamboo-carbon powder by using old bamboo, and with polyester fiber melt spinning
At bamboo charcoal fiber, can have superior fungistatic effect;The adsorption effect for also utilizing the micropore of bamboo charcoal fiber to have, makes mosquito-proof
Agent penetrates into each micropore, and is adsorbed on anophelifuge in the micropore of bamboo charcoal fiber steadily in the long term using thermal finalization, by this
Clothes made of fiber and home textile articles for use, not only to Candida albicans, staphylococcus aureus, Escherichia coli, hay bacillus etc.
Mixed bacteria has high fungistatic effect, but also can expelling mosquito so that human body can be from bite by mosquitos.
Example the above is only the implementation of the present invention is not intended to limit the scope of the invention, every to utilize this hair
Equivalent structure or equivalent flow shift made by bright description is applied directly or indirectly in other relevant technology necks
Domain is included within the scope of the present invention.
Claims (6)
1. a kind of preparation method of the mosquito-proof bacteriostatic fiber of bamboo charcoal, which is characterized in that specifically comprise the following steps:
(1)Old bamboo is selected, and is sintered into bamboo charcoal, the bamboo charcoal is then ground by bamboo charcoal using gas flow crushing process
Powder;
(2)The bamboo-carbon powder is equably spilt into the polyester fiber of melting, if then use arterial highway draft process, until each bamboo
Charcoal powder naked fall obtains bamboo charcoal fiber after polyester fibre surface, spinning;
(3)Ribes after oil expression are selected, are placed on after being dried under high temperature, using gas flow crushing process by the ribes powder
It is extracted after being broken into tea oil slag, obtains anophelifuge;
(4)Bamboo charcoal fiber is crimped using crimping device, and will be prevented by titration mechanism built-in in the crimping device
Mosquito agent drops to bamboo charcoal fiber surface so that anophelifuge is adsorbed in the micropore of bamboo charcoal fiber, eventually passes through 140-160 DEG C of pine
The mosquito-proof bacteriostatic fiber of bamboo charcoal is made after stablizing in relaxation thermal finalization.
2. the preparation method of the mosquito-proof bacteriostatic fiber of bamboo charcoal according to claim 1, which is characterized in that the old bamboo
Age needs 5 years or more.
3. the preparation method of the mosquito-proof bacteriostatic fiber of bamboo charcoal according to claim 1, which is characterized in that the bamboo-carbon powder
Grain size is 300-500 nanometers.
4. the preparation method of the mosquito-proof bacteriostatic fiber of bamboo charcoal according to claim 1, which is characterized in that in the bamboo charcoal fiber
In, the weight percent content of the bamboo-carbon powder is 1-5%.
5. the preparation method of the mosquito-proof bacteriostatic fiber of bamboo charcoal according to claim 1, which is characterized in that the grain of the tea oil slag
Diameter is 150-250 nanometers.
6. the preparation method of the mosquito-proof bacteriostatic fiber of bamboo charcoal according to claim 1, which is characterized in that the mosquito-proof suppression of bamboo charcoal
The fineness of bacterium fiber is 1.5-11D.