CN108212504A - A kind of method that pre-selection-roasting-magnetic floats technique recycling magnetic tailing - Google Patents

A kind of method that pre-selection-roasting-magnetic floats technique recycling magnetic tailing Download PDF

Info

Publication number
CN108212504A
CN108212504A CN201810187067.9A CN201810187067A CN108212504A CN 108212504 A CN108212504 A CN 108212504A CN 201810187067 A CN201810187067 A CN 201810187067A CN 108212504 A CN108212504 A CN 108212504A
Authority
CN
China
Prior art keywords
magnetic
tailing
concentrate
grade
section
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Withdrawn
Application number
CN201810187067.9A
Other languages
Chinese (zh)
Inventor
杨晓峰
刘双安
宋均利
侯卫钢
陈�峰
卢玉明
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Ansteel Mining Co Ltd
Angang Group Mining Co Ltd
Original Assignee
Angang Group Mining Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Angang Group Mining Co Ltd filed Critical Angang Group Mining Co Ltd
Priority to CN201810187067.9A priority Critical patent/CN108212504A/en
Publication of CN108212504A publication Critical patent/CN108212504A/en
Withdrawn legal-status Critical Current

Abstract

The present invention relates to a kind of methods for preselecting roasting magnetic and floating technique recycling magnetic tailing, include the following steps:It is 9 ~ 13% by Iron grade, carbonic acid iron content is more than 3% magnetic tailing, feed one section of weak magnetic, one magnetic tail feeds one section of strong magnetic, the last one essence feeds the spiral chute reselection operation of a thick essence, smart spiral shell tail merges into preliminary rejection with thick spiral shell tail and the last one tail, and smart spiral shell essence and a magnetic essence merge into pre- concentrate selection;Pre- concentrate selection is concentrated, filter, roasting obtains roasted ore;Roasted ore is through closed circuit grinding, the overflow product of 0.046mm contents 83%~90% feeds two sections of weak magnetics, two magnetic essences feed the reverse flotation work that a thick essence three is swept, concentrate through reverse flotation is the final concentrate of more than 65% grade, and centrifuge tailing and two magnetic tail ore deposits, preliminary rejection merge into the true tailings of grade 7%~10%.It is an advantage of the invention that:1. pre-selection is without ore grinding;2. magnetic separation is combined with reverse flotation, regrind granularity and put slightly, yield improves.

Description

A kind of method that pre-selection-roasting-magnetic floats technique recycling magnetic tailing
Technical field
The invention belongs to technical field of beneficiation, and in particular to the magnetic tailing that carbonic acid iron content is more than 3% is sorted A kind of pre-selection-roasting-magnetic heavy industry skill recycling magnetic tailing method.
Background technology
The method recycled at present to magnetic tailing of the valuable mineral based on Armco magnetic iron mineral, it is common that using magnetic Choosing-dusting cover-magnetic separation process or single magnetic separation process are sorted, and the Armco magnetic iron mineral in magnetic tailing are returned so as to reach It receives, obtains the purpose of qualified iron ore concentrate.The selection of single magnetic separation process or magnetic separation-dusting cover-magnetic separation process is according to magnetic tailing The size of middle Armco magnetic iron mineral disseminated grain size and it is determining, be specifically summarized as follows:
Magnetic separation-dusting cover-magnetic separation process:
For Armco magnetic iron mineral disseminated grain size in magnetic tailing more than 30 particles, regrind granularity -0.074mm contents 95% with Under magnetic tailing, magnetic separation-dusting cover-magnetic separation process generally can be used, it is common that throwing tail is carried out using disc type recycling machine first, so It after being regrinded afterwards to recycling machine concentrate, then carries out weak magnetic machine and sorts, weak magnetic machine concentrate feeds dusting cover, and dusting cover undersize passes through again Become final concentrate after weak magnetic machine is selected, it is weak that the return of dusting cover oversize feeds weak magnetic machine-dusting cover-again after regrinding or individually regrinding Magnetomechanical is sorted, and is formed closed circuit;
Single magnetic separation process:
For Armco magnetic iron mineral disseminated grain size in magnetic tailing in 30 particles hereinafter, regrind granularity -0.046mm contents 90% with On magnetic tailing, single magnetic separation process generally can be used, it is common that throwing tail is carried out using disc type recycling machine first, then to return After receipts machine concentrate is regrinded, then combined using multistage magnetic separator or dehydration slot and magnetic separator and sort acquisition concentrate.
For iron mineral disseminated grain size at 0 ~ 30 micron, regrind particulate magnetic of the granularity in more than 90% -0.046mm contents Iron ore mine, the major defect sorted using single magnetic separation process or magnetic separation-dusting cover-magnetic separation process are:
1)Magnetic concentration working regrind granularity it is meticulous when be easy to cause magnetism and be mingled with, high-grade concentrate can not be obtained;2)Regrind granularity It is meticulous, mutually in requisition for thinner dusting cover screen size, sieve pore blockade is easily caused in production;Otherwise, need relatively low dusting cover to Ore deposit concentration and larger flushing water, are not easy to realize in production.
The method that the synthesis tailing of the bloodstone to valuable mineral based on weak magnetism mineral is recycled at present, recycling Rate it is higher be pre-selection-calcining magnetic separation process, pre-selection technique is generally using magnetic separation-regrind-magnetic separation process, and specific summary is such as Under:
The high intensity magnetic mineral that comprehensive tailing obtains after one section of high-intensity magnetic separation feeds grinding classification system, and ore milling product is strong through two sections again Magnetic separation is other, and the last two essence is concentrated, carries out reduction roasting after filtering, and product is sorted through weak magnetic after roasting, and inferior fine magnetite concentrate is again through ore grinding Afterwards, then using weak magnetic selected, acquisition final concentrate is carried out.
Carbonic acid iron content is higher in the magnetic iron ore of part valuable mineral fine-grained disseminated grain at present, reaches more than 3%.Magneticore-dressing plant adopts Such magnetic iron ore is handled with the single magnetic separation technological process of production, ferric carbonate substantially enters magnetic tailing.To such magnetic tailing Recovery process and method, particularly to the recovery process of ferric carbonate and method carry out further investigation inquire into have realistic meaning.
The recovery process of the existing above-mentioned magnetic tailing to valuable mineral based on Armco magnetic iron mineral is used, it is not only magnetic Iron recovery is relatively low, and can not recycle the ferric carbonate being lost in tailing completely;
The recovery process of the synthesis tailing of the existing above-mentioned bloodstone to valuable mineral based on weak magnetism mineral is used, Pre-selection technique is magnetic separation-regrind-magnetic separation, recycles the ferric carbonate in magnetic tailing using strong magnetic, regrinds front and rear two sections of high intensity magnetic minerals Grade compared with to ore deposit, a strong concentrate concentrate 15% hereinafter, two strong concentrate concentrates 21% hereinafter, increase rate is minimum, as a result pay no attention to Think;Then it is reasonable using roasting technique, ferric carbonate can be converted into Armco magnetic iron, but follow-up low intensity magnetic separation operation will obtain grade 65% iron ore concentrate, -500 more than 97% mesh will be reached by regrinding granularity, regrind that granularity requirements are too thin, and cost is high, and are difficult to realize Commercial Application.
Invention content
The object of the present invention is to provide a kind of pre-selection-roastings sorted to the magnetic tailing that carbonic acid iron content is more than 3% The method that burning-magnetic floats technique recycling magnetic tailing.
The invention is realized in this way.
The method that a kind of pre-selection-roasting-magnetic of the present invention floats technique recycling magnetic tailing, includes the following steps:
1)One section of weak magnetic will will be fed containing the magnetic tailing of carbonic acid iron, and obtain one section of weak magnetic essence that grade is 25%~30% Ore deposit and one section of weakly magnetic tailings;One section of weakly magnetic tailings is fed into one section of strong magnetic, obtains one section of high intensity magnetic mineral that grade is 12%~14% With the one section strong magnetic tail ore deposit that grade is 5%~7%;
2)One section of high intensity magnetic mineral is fed into roughing spiral chute, thick spiral shell concentrate feeds selected spiral chute, obtains selected spiral and slips Slot concentrate, selected spiral chute chats and selected spiral chute tailing, the selected selected spiral chute of spiral chute middling recurrence, essence Spiral chute tailing is selected to form preliminary rejection with roughing spiral chute tailing and one section strong magnetic tail ore deposit and throws tail, grade is 55%~60% Selected spiral chute concentrate and one section of inferior fine magnetite concentrate merge into pre- concentrate selection, pre-selection concentrate grade is 37%~42%;
3)Pre- concentrate selection is fed into concentrator concentration, thickener underflow feeds filter filtering, and it is 10% to obtain moisture weight content ~ 15% filter cake, then filter cake restored under the conditions of 530 DEG C ~ 570 DEG C of temperature by roasting technique, obtain Armco magnetic iron distributive law More than 85% roasted ore;Concentrator overflow and filter filtrate are as recycling water utilization;
4)Roasted ore is fed to the closed circuit grinding system of cyclone and ball mill composition, partition size is -0.046mm contents 83% ~90% closed circuit grinding overflow product feeds two sections of weak magnetics, obtains two sections of inferior fine magnetite concentrates and two sections of weakly magnetic tailings, two sections of weak magnetic essences Ore deposit feeds the reverse floatation process that a thick essence three is swept, and concentrate through reverse flotation is final concentrate, reverse flotation tailing and two sections of weakly magnetic tailings, Preliminary rejection merges into true tailings.
Iron grade in the magnetic tailing containing carbonic acid iron is 9 ~ 13%, and carbonic acid iron content is more than 3%.
The final concentrate grade more than 65%, true tailings grade be 7%~10%.
Reverse floatation agent is added in by the sequence of regulator, inhibitor, activator, collecting agent.
It is an advantage of the invention that:
1. not having grinding operation in pre-selection technique, ore grinding cost is saved, advance concentrate grade is high, is 37%~42%, and low yield is 8% ~ 10%, reduce follow-up more than 50% roasting sorting operation cost;
2. ferric carbonate is converted into Armco magnetic iron mineral by carbonic acid iron content more than 3% using roasting technique in magnetic tailing, realize Itself and the common recycling for the Armco magnetic iron mineral being lost in tailing, the rate of recovery improve;
3. pair roasted ore is sorted using weak magnetic with reverse flotation group technology, it is desirable that granularity of regrinding put and slightly contain for -0.045mm Amount 83%~90%, is industrially easily achieved.
Description of the drawings
Fig. 1 is that pre-selection-roasting-magnetic floats the method flow diagram that technique recycles magnetic tailing.
Specific embodiment
The invention will be further described with reference to the accompanying drawings and examples.
As shown in Figure 1:
Embodiment 1:
The method that a kind of pre-selection-roasting-magnetic of the present invention floats technique recycling magnetic tailing, includes the following steps:
1)It is 10.46% by Iron grade, carbonic acid iron content is 3.5% magnetic tailing, feeds one section of weak magnetic, obtains grade and is 27.35% one section of inferior fine magnetite concentrate and one section of weakly magnetic tailings;One section of weakly magnetic tailings is fed into one section of strong magnetic, obtaining grade is 12.65% one section of high intensity magnetic mineral and grade is 5.92% one section strong magnetic tail ore deposit;
2)One section of high intensity magnetic mineral is fed into roughing spiral chute, thick spiral shell concentrate feeds selected spiral chute, obtains selected spiral and slips Slot concentrate, selected spiral chute chats and selected spiral chute tailing, the selected selected spiral chute of spiral chute middling recurrence, essence Spiral chute tailing is selected to form preliminary rejection with roughing spiral chute tailing and one section strong magnetic tail ore deposit and throws tail, grade is 57.12% Selected spiral chute concentrate and one section of inferior fine magnetite concentrate merge into pre- concentrate selection, and pre-selection concentrate grade is 38.96%;
3)Pre- concentrate selection is fed into concentrator concentration, thickener underflow feeds filter filtering, and it is 10% to obtain moisture weight content ~ 15% filter cake, then filter cake restored under the conditions of 530 DEG C ~ 570 DEG C of temperature by roasting technique, obtain Armco magnetic iron distributive law More than 85% roasted ore;Concentrator overflow and filter filtrate are as recycling water utilization;
4)Roasted ore is fed to the closed circuit grinding system of cyclone and ball mill composition, partition size is -0.046mm contents 89.5% closed circuit grinding overflow product feeds two sections of weak magnetics, obtains two sections of inferior fine magnetite concentrates and two sections of weakly magnetic tailings, two sections of weak magnetic essences Ore deposit feeds the reverse floatation process that a thick essence three is swept, and concentrate through reverse flotation is the final concentrate of grade 65.18%, reverse flotation tailing with Two sections of weakly magnetic tailings, preliminary rejection merge into true tailings, and true tailings grade is 8.26%.
Embodiment 2:
The method that a kind of pre-selection-roasting-magnetic of the present invention floats technique recycling magnetic tailing, includes the following steps:
1)It is 12.13% by Iron grade, carbonic acid iron content is 4.23% magnetic tailing, feeds one section of weak magnetic, obtains grade and is 28.01% one section of inferior fine magnetite concentrate and one section of weakly magnetic tailings;One section of weakly magnetic tailings is fed into one section of strong magnetic, obtaining grade is 13.62% one section of high intensity magnetic mineral and grade is 6.53% one section strong magnetic tail ore deposit;
2)One section of high intensity magnetic mineral is fed into roughing spiral chute, thick spiral shell concentrate feeds selected spiral chute, obtains selected spiral and slips Slot concentrate, selected spiral chute chats and selected spiral chute tailing, the selected selected spiral chute of spiral chute middling recurrence, essence Spiral chute tailing is selected to form preliminary rejection with roughing spiral chute tailing and one section strong magnetic tail ore deposit and throws tail, grade is 57.86% Selected spiral chute concentrate and one section of inferior fine magnetite concentrate merge into pre- concentrate selection, and pre-selection concentrate grade is 37.86%;
3)Pre- concentrate selection is fed into concentrator concentration, thickener underflow feeds filter filtering, and it is 10% to obtain moisture weight content ~ 15% filter cake, then filter cake restored under the conditions of 530 DEG C ~ 570 DEG C of temperature by roasting technique, obtain Armco magnetic iron distributive law More than 85% roasted ore;Concentrator overflow and filter filtrate are as recycling water utilization;
4)Roasted ore is fed to the closed circuit grinding system of cyclone and ball mill composition, partition size is -0.046mm contents 83.5% closed circuit grinding overflow product feeds two sections of weak magnetics, obtains two sections of inferior fine magnetite concentrates and two sections of weakly magnetic tailings, two sections of weak magnetic essences Ore deposit feeds the reverse floatation process that a thick essence three is swept, and concentrate through reverse flotation is the final concentrate of grade 65.33%, reverse flotation tailing with Two sections of weakly magnetic tailings, preliminary rejection merge into true tailings, and true tailings grade is 9.05%.

Claims (4)

1. a kind of method that pre-selection-roasting-magnetic floats technique recycling magnetic tailing, it is characterised in that include the following steps:
1)One section of weak magnetic will will be fed containing the magnetic tailing of carbonic acid iron, and obtain one section of weak magnetic essence that grade is 25%~30% Ore deposit and one section of weakly magnetic tailings;One section of weakly magnetic tailings is fed into one section of strong magnetic, obtains one section of high intensity magnetic mineral that grade is 12%~14% With the one section strong magnetic tail ore deposit that grade is 5%~7%;
2)One section of high intensity magnetic mineral is fed into roughing spiral chute, thick spiral shell concentrate feeds selected spiral chute, obtains selected spiral and slips Slot concentrate, selected spiral chute chats and selected spiral chute tailing, the selected selected spiral chute of spiral chute middling recurrence, essence Spiral chute tailing is selected to form preliminary rejection with roughing spiral chute tailing and one section strong magnetic tail ore deposit and throws tail, grade is 55%~60% Selected spiral chute concentrate and one section of inferior fine magnetite concentrate merge into pre- concentrate selection, pre-selection concentrate grade is 37%~42%;
3)Pre- concentrate selection is fed into concentrator concentration, thickener underflow feeds filter filtering, and it is 10% to obtain moisture weight content ~ 15% filter cake, then filter cake restored under the conditions of 530 DEG C ~ 570 DEG C of temperature by roasting technique, obtain Armco magnetic iron distributive law More than 85% roasted ore;Concentrator overflow and filter filtrate are as recycling water utilization;
4)Roasted ore is fed to the closed circuit grinding system of cyclone and ball mill composition, partition size is -0.046mm contents 83% ~90% closed circuit grinding overflow product feeds two sections of weak magnetics, obtains two sections of inferior fine magnetite concentrates and two sections of weakly magnetic tailings, two sections of weak magnetic essences Ore deposit feeds the reverse floatation process that a thick essence three is swept, and concentrate through reverse flotation is final concentrate, reverse flotation tailing and two sections of weakly magnetic tailings, Preliminary rejection merges into true tailings.
2. the method that pre-selection-roasting-magnetic according to claim 1 floats technique recycling magnetic tailing, it is characterised in that described The magnetic tailing containing carbonic acid iron in Iron grade for 9 ~ 13%, carbonic acid iron content is more than 3%.
3. the method that pre-selection-roasting-magnetic according to claim 1 floats technique recycling magnetic tailing, it is characterised in that described Final concentrate grade more than 65%, true tailings grade be 7%~10%.
4. a kind of method that pre-selection-roasting-magnetic floats technique recycling magnetic tailing according to claim 1, it is characterised in that anti- Floating agent is added in by the sequence of regulator, inhibitor, activator, collecting agent.
CN201810187067.9A 2018-03-07 2018-03-07 A kind of method that pre-selection-roasting-magnetic floats technique recycling magnetic tailing Withdrawn CN108212504A (en)